Extruded Polystyrene Foam: Propylene-Blown Log Let Out at 50 °C (McIntire, Dow 1948, Ex. 3, Test 2)

Extruded polystyrene foam blown with a propylene gas fraction instead of methyl chloride. Polystyrene stands two days at 40 °C with the propylene under pressure and becomes a gel. Let out at 50 °C (250 psi in the tower), it swelled into a log 6 to 9 inches across, weighing 4.8 lb per cubic foot, with somewhat smaller, uniform cells. Source: O. R. McIntire (Dow), US 2,450,436 (1948), Example 3. Picture: the patent's drawing.
Lanjutan
3 days

Arahan

1

Charge the tower with polystyrene

Charge a high-pressure tower with 300 lb of granular polystyrene.

Bahan untuk langkah ini:

PolistirenaPolistirena300 paun

Alatan diperlukan:

Reaktor bertekananReaktor bertekanan
Neraca dua piringNeraca dua piring
Sarung tangan getahSarung tangan getah
2

Add the propylene fraction

Add 100 lb of a cracked-oil gas fraction that is about 93 % propylene, under pressure, and close the tower. Propylene is a flammable gas: no flames, strong ventilation.

Bahan untuk langkah ini:

PropilenaPropilena100 paun

Alatan diperlukan:

Silinder gas bertekananSilinder gas bertekanan
Reaktor bertekananReaktor bertekanan
Gogal Percikan KimiaGogal Percikan Kimia
3

Stand two days at 40 °C

Let the tower stand for two days at 40 °C while the polystyrene takes up the propylene.

Alatan diperlukan:

Reaktor bertekananReaktor bertekanan
Termometer MakmalTermometer Makmal
4

Let it out at 50 °C

Open the valved outlet near the bottom (3.25 inch in the patent) at 50 °C. The pressure is about 250 psi. The gel flows out and swells into a log 6 to 9 inches across, 4.8 lb per cubic foot, with somewhat smaller, uniform cells. Close the outlet again. The patent heated step by step (50, 60, 75 °C) for several hours each, letting a portion out at each step.

Alatan diperlukan:

Reaktor bertekananReaktor bertekanan
Termometer MakmalTermometer Makmal
Gogal Percikan KimiaGogal Percikan Kimia
Sarung tangan getahSarung tangan getah
5

Saw into boards

When the foam has set, saw it lengthwise into slabs (ours: a woodworking saw).

Alatan diperlukan:

Gergaji tukang kayuGergaji tukang kayu
Sarung tangan getahSarung tangan getah

Bahan

2
  • 300 paun
    Pemegang Tempat
  • 100 paun
    Pemegang Tempat

Alatan Diperlukan

7

CC0 Domain Awam

Blueprint ini dikeluarkan di bawah CC0. Anda bebas menyalin, mengubah, mengedar, dan menggunakan karya ini untuk sebarang tujuan, tanpa meminta kebenaran.

Sokong Pembuat dengan membeli produk melalui Blueprint mereka di mana mereka memperoleh Komisen Pembuat ditetapkan oleh Penjual, atau cipta iterasi baru Blueprint ini dan sertakan ia sebagai sambungan dalam Blueprint anda sendiri untuk berkongsi hasil.

Perbincangan

(0)

Log masuk untuk menyertai perbincangan

Memuatkan komen...