Ferrite Toroid Core: Magnesium-Zinc Ferrite Reheated 18 h at 1000 °C and 20 h at 750 °C (Snoek 1948, Ex. III)
Charlie

Dicipta oleh

Charlie

28. Oktober 2026DE
10
0
0
0
0

Ferrite Toroid Core: Magnesium-Zinc Ferrite Reheated 18 h at 1000 °C and 20 h at 750 °C (Snoek 1948, Ex. III)

Snoek's magnesium-zinc ferrite ring (Example III), fired at 1400 °C and then given a second long treatment in oxygen: 18 hours at 1000 °C and 20 hours at 750 °C. He measured how its losses change with frequency, but gives no permeability for the reheated core. Source: J. L. Snoek, US 2,452,529 (Philips, 1948), Example III. Picture: our diagram.
Lanjutan
3 days

Arahan

1

Weigh 28 : 18 : 54 mol %

Mix 28 mol % magnesium oxide, 18 mol % zinc oxide and 54 mol % ferric oxide. Ours, by weight: 10.06 g magnesium oxide, 13.06 g zinc oxide and 76.88 g ferric oxide per 100 g.

Bahan untuk langkah ini:

Magnesium oksidaMagnesium oksida10.06 g
Serbuk Zink OksidaSerbuk Zink Oksida13.06 g
Ferik OksidaFerik Oksida76.88 g

Alatan diperlukan:

Neraca dua piringNeraca dua piring
Topeng HabukTopeng Habuk
2

Grind 30 hours in an iron mill

Grind the mixture for 30 hours in an iron ball mill.

Alatan diperlukan:

Kilang Bebola BesiKilang Bebola Besi
Topeng HabukTopeng Habuk
3

Mould a ring at 4 tons per cm²

Mould the powder at 4 tons per square centimetre into a ring 3 cm across with a 4 × 4 mm section.

Alatan diperlukan:

Mesin tekan hidraulikMesin tekan hidraulik
Acuan Penekan GelangAcuan Penekan Gelang
Topeng HabukTopeng Habuk
4

Fire 2 hours at 1400 °C, cool 5–10 °C a minute

Heat the ring in oxygen for 2 hours at 1400 °C and cool it slowly in oxygen at 5 to 10 °C per minute.

Alatan diperlukan:

Relau TiubRelau Tiub
OksigenOksigen
Silinder gas bertekananSilinder gas bertekanan
PirometerPirometer
Penyepit Mangkuk PijarPenyepit Mangkuk Pijar
Sarung Tangan Tahan HabaSarung Tangan Tahan Haba
5

Reheat: 18 hours at 1000 °C, 20 hours at 750 °C

Heat the cooled core to 1000 °C and hold it there for 18 hours, then at 750 °C for 20 hours, and cool slowly again, all in oxygen. Snoek shows the resulting losses only as a curve; he gives no permeability for it.

Alatan diperlukan:

Relau TiubRelau Tiub
OksigenOksigen
Silinder gas bertekananSilinder gas bertekanan
PirometerPirometer
Penyepit Mangkuk PijarPenyepit Mangkuk Pijar
Sarung Tangan Tahan HabaSarung Tangan Tahan Haba

Bahan

3

Alatan Diperlukan

11

Blueprint berkaitan

Blueprint ini berkongsi pengetahuan — teknik, bahan atau prinsip

CC0 Domain Awam

Blueprint ini dikeluarkan di bawah CC0. Anda bebas menyalin, mengubah, mengedar, dan menggunakan karya ini untuk sebarang tujuan, tanpa meminta kebenaran.

Sokong Pembuat dengan membeli produk melalui Blueprint mereka di mana mereka memperoleh Komisen Pembuat ditetapkan oleh Penjual, atau cipta iterasi baru Blueprint ini dan sertakan ia sebagai sambungan dalam Blueprint anda sendiri untuk berkongsi hasil.

Perbincangan

(0)

Log masuk untuk menyertai perbincangan

Memuatkan komen...