Ferromolybdenum: Molybdic Oxide Smelted with Coke and Lime into Molten Steel in an Electric Arc Furnace (Brigham, US 4,160,661)
Charlie

Dicipta oleh

Charlie

1. November 2026DE
7
0
0
0
0

Ferromolybdenum: Molybdic Oxide Smelted with Coke and Lime into Molten Steel in an Electric Arc Furnace (Brigham, US 4,160,661)

Technical molybdic oxide is fed in cans, with coke and lime, into a bath of molten steel in a 3000 kVA arc furnace. The electrodes stay in the slag, and the coke is trimmed after every charge unit so the metal keeps under 0.1 % carbon. Ferrosilicon and lime strip the slag, and the metal is shotted in running water. Result: from 5000 lb oxide, 3110 lb shot and pig of 54.1 % molybdenum, 0.06 % carbon, 43.1 % iron (Heat 4), using 1.94 kWh per lb of molybdenum. Source: Brigham, Sirianni and Garner, US patent 4,160,661 (1979), Example 2, Heat 4. Not given: how the shot was heated while drying overnight. Picture drawn by Youblob.
Lanjutan
1 day

Arahan

1

Melt the steel

In a three-phase 3000 kVA arc furnace with 8 in graphite electrodes, lined with magnesia brick and rammed basic refractory (about 60 % MgO), 5 ft 6 in across and 26 in deep below the tap hole, melt 812 lb steel plate with 80 lb burnt lime under full power. Lead the fume to a bag house.

Bahan untuk langkah ini:

Plat keluli lembutPlat keluli lembut812 paun

Alatan diperlukan:

Kapur tohorKapur tohor
Relau arka elektrikRelau arka elektrik
Elektrod grafitElektrod grafit
Rumah penapis begRumah penapis beg
2

Make up the charge units

While it melts, weigh out five charge units, each 1000 lb molybdic oxide (in cans of 37 lb oxide in a 2 lb steel can), 250 lb coke and 320 lb lime. For Heat 4 that was 5000 lb oxide, 1150 lb coke, 1600 lb lime and 1488 lb steel in plate and cans. Ours: metallurgical coke for the dried breeze coke.

Bahan untuk langkah ini:

Oksida molibdenum teknikalOksida molibdenum teknikal5000 paun
Plat keluli lembutPlat keluli lembut1488 paun

Alatan diperlukan:

Kok metalurgiKok metalurgi
Kapur tohorKapur tohor
Penimbang pelantar industriPenimbang pelantar industri
3

Smelt in the bath

When the bath is molten at about 1450 °C, add one can of oxide with equal shovels of coke and lime every 2 minutes, about 1 hour per unit. Use the 205 V tap so the electrodes dip only into the slag; hold the bath at most 1760 °C. About 1 kWh per lb of oxide.

Alatan diperlukan:

PenyodokPenyodok
Relau arka elektrikRelau arka elektrik
4

Keep the carbon down

After every charge unit, dip a steel spoon into the bath and analyse the carbon (about 15 minutes); cut the coke so the metal stays below 0.1 % carbon.

Alatan diperlukan:

Kok metalurgiKok metalurgi
5

Strip the slag and tap

Add 200 lb ferrosilicon and 560 lb lime to strip the slag. Tip the furnace into a preheated 5000 lb ladle: the first ladle is mostly slag, the second mostly metal. Back-pour the slag into slag pots.

Alatan diperlukan:

FerosilikonFerosilikon
Kapur tohorKapur tohor
Cedok tuang logamCedok tuang logam
6

Shot the metal

Pour the metal from the ladle into a second unlined 5000 lb ladle filled with running water from a 2 1/4 in fire hose, about 3000 lb a minute, from about 4 ft up; 2000 lb shots in 10 to 15 minutes. Dry the shot overnight at about 300 °F in 40 gallon drums. Ours: a drying oven.

Alatan diperlukan:

Cedok tuang logamCedok tuang logam
AirAir
Ketuhar pengeringanKetuhar pengeringan

Bahan

2

Alatan Diperlukan

11

CC0 Domain Awam

Blueprint ini dikeluarkan di bawah CC0. Anda bebas menyalin, mengubah, mengedar, dan menggunakan karya ini untuk sebarang tujuan, tanpa meminta kebenaran.

Sokong Pembuat dengan membeli produk melalui Blueprint mereka di mana mereka memperoleh Komisen Pembuat ditetapkan oleh Penjual, atau cipta iterasi baru Blueprint ini dan sertakan ia sebagai sambungan dalam Blueprint anda sendiri untuk berkongsi hasil.

Perbincangan

(0)

Log masuk untuk menyertai perbincangan

Memuatkan komen...