Iron Sheet Hammered Out from Bar

Before rolling mills, iron plate for cauldrons and griddles was hammered out of bar by hand. The bar is spread sideways with the hammer's peen, flattened with the face, then planished with a flatter until it is an even sheet two to three millimetres thick. The picture: a cauldron of riveted iron plates from Vendel, Uppland, Sweden (Swedish History Museum, SHM 7250:XI).
Lanjutan
A day

Arahan

1

Heat the bar

Bring the wrought iron bar to a bright yellow-orange.

Bahan untuk langkah ini:

Bar besi tempaBar besi tempa1 kg
ArangArang1 as required

Alatan diperlukan:

Relau tukang besiRelau tukang besi
Penyepit tukang besiPenyepit tukang besi
Sarung tangan kimpalanSarung tangan kimpalan
Cermin mata keselamatanCermin mata keselamatan
2

Spread it with the peen

Strike with the cross peen running along the bar, so the grooves push the metal out sideways. Flatten the ridges with the face. Turn it over and repeat. Reheat as soon as it dulls.

Alatan diperlukan:

AndasAndas
Tukul kepala baji lintangTukul kepala baji lintang
Penyepit tukang besiPenyepit tukang besi
Sarung tangan kimpalanSarung tangan kimpalan
Cermin mata keselamatanCermin mata keselamatan
3

Thin it evenly

Work outward from the middle, peen then face, until the plate is about 3 mm. Fold nothing: a fold will not weld back flat.

Alatan diperlukan:

Relau tukang besiRelau tukang besi
AndasAndas
Tukul kepala baji lintangTukul kepala baji lintang
Sarung tangan kimpalanSarung tangan kimpalan
Cermin mata keselamatanCermin mata keselamatan
4

Planish with a flatter

With a helper on the sledge, set the flatter on the hot plate and planish the hammer marks out. Check it flat with a straight edge and the thickness with the caliper.

Alatan diperlukan:

Perata tempaanPerata tempaan
Tukul besarTukul besar
AndasAndas
Pembaris pelurusPembaris pelurus
Angkup Digital 6 InciAngkup Digital 6 Inci
Sarung tangan kimpalanSarung tangan kimpalan
Cermin mata keselamatanCermin mata keselamatan
5

Trim the edges

Cut ragged edges off with a cold chisel on the anvil while it is still warm.

Alatan diperlukan:

Pahat besi sejukPahat besi sejuk
AndasAndas
Tukul kepala baji lintangTukul kepala baji lintang
Sarung tangan kimpalanSarung tangan kimpalan
Cermin mata keselamatanCermin mata keselamatan
6

How much sheet a bar gives

Memuatkan buku nota Jupyter…

Bahan

2
  • Pemegang Tempat
  • 1 as required
    Pemegang Tempat

Alatan Diperlukan

11

CC0 Domain Awam

Blueprint ini dikeluarkan di bawah CC0. Anda bebas menyalin, mengubah, mengedar, dan menggunakan karya ini untuk sebarang tujuan, tanpa meminta kebenaran.

Sokong Pembuat dengan membeli produk melalui Blueprint mereka di mana mereka memperoleh Komisen Pembuat ditetapkan oleh Penjual, atau cipta iterasi baru Blueprint ini dan sertakan ia sebagai sambungan dalam Blueprint anda sendiri untuk berkongsi hasil.

Perbincangan

(0)

Log masuk untuk menyertai perbincangan

Memuatkan komen...