Lactide: Lactic Acid Condensed and Cracked under Vacuum, Recrystallised
Charlie

Dicipta oleh

Charlie

19. Oktober 2026DE
18
0
0
0
0

Lactide: Lactic Acid Condensed and Cracked under Vacuum, Recrystallised

Lactide is the ring-shaped double molecule of lactic acid, the monomer from which PLA is made. Schneider's du Pont patent (US 2,703,316, 1955) drives the water out of lactic acid, condenses it under vacuum to a syrupy low polymer, then heats that to 200–250 °C at 8–10 mm so that lactide distils off. For a tough plastic it must be very pure: recrystallise it from ethyl acetate until it melts at 120 °C or higher (best 123–125 °C). The picture: our diagram.
Lanjutan
1–2 days

Arahan

1

Drive off the water

Distil the lactic acid at atmospheric pressure at 120–130 °C until nearly all the water of dilution has gone.

Bahan untuk langkah ini:

Asid Laktik (teknikal)Asid Laktik (teknikal)1 keping

Alatan diperlukan:

Kelalang dasar bulatKelalang dasar bulat
Gegelung kondenserGegelung kondenser
Plat PemanasPlat Pemanas
Rendaman MinyakRendaman Minyak
Termometer MakmalTermometer Makmal
2

Condense under vacuum

Continue distilling under 17–35 mm of mercury. Water of esterification comes off and the acid becomes a syrupy low polymer (polylactic acid).

Alatan diperlukan:

Pam vakumPam vakum
Tolok vakumTolok vakum
Perangkap SejukPerangkap Sejuk
Rendaman MinyakRendaman Minyak
Termometer MakmalTermometer Makmal
3

Crack to lactide

Lower the pressure to 8–10 mm and raise the temperature to 200–250 °C. Lactide distils at 130–140 °C (10–13 mm) and sets to a soft crystalline solid.

Alatan diperlukan:

Pam vakumPam vakum
Tolok vakumTolok vakum
Gegelung kondenserGegelung kondenser
Rendaman MinyakRendaman Minyak
Termometer MakmalTermometer Makmal
Sarung Tangan Tahan HabaSarung Tangan Tahan Haba
4

Recrystallise from ethyl acetate

Recrystallise the crude lactide from ethyl acetate, filter and dry. Repeat: in the patent the melting point rose from 114–115 °C after the first crystallisation to 118, 123–124 and 124–125 °C after the fourth.

Alatan diperlukan:

Etil AsetatEtil Asetat
Bikar Kaca Tahan HabaBikar Kaca Tahan Haba
Plat PemanasPlat Pemanas
Corong Büchner (porselin)Corong Büchner (porselin)
Kertas TurasKertas Turas
Gogal Percikan KimiaGogal Percikan Kimia
5

Check the melting point

Put a few crystals in a capillary tube and warm slowly. Lactide melting at 120 °C or above is fit for making PLA; below 120 °C it gives a brittle polymer.

Alatan diperlukan:

Tiub kapilari kacaTiub kapilari kaca
Termometer MakmalTermometer Makmal
Rendaman MinyakRendaman Minyak

Bahan

1

Alatan Diperlukan

15

Blueprint ini membuat

CC0 Domain Awam

Blueprint ini dikeluarkan di bawah CC0. Anda bebas menyalin, mengubah, mengedar, dan menggunakan karya ini untuk sebarang tujuan, tanpa meminta kebenaran.

Sokong Pembuat dengan membeli produk melalui Blueprint mereka di mana mereka memperoleh Komisen Pembuat ditetapkan oleh Penjual, atau cipta iterasi baru Blueprint ini dan sertakan ia sebagai sambungan dalam Blueprint anda sendiri untuk berkongsi hasil.

Perbincangan

(0)

Log masuk untuk menyertai perbincangan

Memuatkan komen...