Strontium Ferrite Disc Magnet: Example 8 Without the Orienting Field (Gorter, Philips 1956, Ex. 8 Comparison)

Made as in Example 8 but without the first, orienting field. Gorter's comparison block held 2,020 gauss with a coercive force of 3,225 oersted and a (BH)max of 0.99 × 10⁶. Source: E. W. Gorter, G. W. Rathenau and A. L. Stuyts (Philips), US 2,762,778 (1956), Example 8. They made blocks; disc size is ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Lanjutan
3 days

Arahan

1

Weigh strontium carbonate and iron oxide

Weigh 29.5 g strontium carbonate and 179 g ferric oxide.

Bahan untuk langkah ini:

Strontium karbonatStrontium karbonat29.5 g
Ferik OksidaFerik Oksida179 g

Alatan diperlukan:

Neraca dua piringNeraca dua piring
Alat Pernafasan P100Alat Pernafasan P100
2

Mill 15 hours with alcohol, dry

Grind in a ball mill with alcohol for 15 hours. Remove the alcohol and dry the powder.

Alatan diperlukan:

Kilang Bebola BesiKilang Bebola Besi
Etanol mutu makmal, 95 %Etanol mutu makmal, 95 %
Ketuhar pengeringanKetuhar pengeringan
3

Pre-fire 2 hours at 1000 °C in air

Heat the powder for 2 hours at 1000 °C in an electric furnace in air. Let it cool.

Alatan diperlukan:

Relau MuffleRelau Muffle
Mangkuk pijar bertutup (porselin)Mangkuk pijar bertutup (porselin)
Penyepit Mangkuk PijarPenyepit Mangkuk Pijar
Sarung Tangan Tahan HabaSarung Tangan Tahan Haba
4

Grind 4 hours in an agate centrifugal mill

Grind the cooled material for 4 hours with alcohol in an agate centrifugal mill, then dry it. This is the pre-fired powder.

Alatan diperlukan:

Pengisar emparan batu akikPengisar emparan batu akik
Etanol mutu makmal, 95 %Etanol mutu makmal, 95 %
Ketuhar pengeringanKetuhar pengeringan
5

Stir into 8 % polyvinyl acetate in acetone

Dissolve polyvinyl acetate in acetone to a 8 % solution and stir the pre-fired powder into it, 1 cc of solution per gram of powder. The binder burns off later.

Alatan diperlukan:

Polivinil AsetatPolivinil Asetat
AsetonAseton
Neraca dua piringNeraca dua piring
6

Mould without a first field

Put the suspension in a moulding die and remove the binder solution without any magnetic field. This is the patent's comparison block.

Alatan diperlukan:

Acuan tekan cakeraAcuan tekan cakera
Mesin tekan hidraulikMesin tekan hidraulik
7

Heat to 500 °C in a 2000 oersted field

Put the block in an electric furnace between the magnet's poles. With a second field of 2000 oersted along the first field's direction, heat to 500 °C, which burns off the rest of the binder. Then switch the field off.

Alatan diperlukan:

Relau TiubRelau Tiub
ElektromagnetElektromagnet
Sarung Tangan Tahan HabaSarung Tangan Tahan Haba
8

Sinter: through a 1280 °C zone in 5 minutes

Pass the block at 20 mm per minute through an electric furnace in air at 1280 °C with a 10 cm hot zone: about 5 minutes in the heat.

Alatan diperlukan:

Relau TiubRelau Tiub
Sarung Tangan Tahan HabaSarung Tangan Tahan Haba
9

Magnetise the block

Magnetise the block in a field. Without the orienting field it has no preferred direction. Ours: an electromagnet. Find the north face with a compass.

Alatan diperlukan:

ElektromagnetElektromagnet
KompasKompas

Bahan

2

Alatan Diperlukan

17

CC0 Domain Awam

Blueprint ini dikeluarkan di bawah CC0. Anda bebas menyalin, mengubah, mengedar, dan menggunakan karya ini untuk sebarang tujuan, tanpa meminta kebenaran.

Sokong Pembuat dengan membeli produk melalui Blueprint mereka di mana mereka memperoleh Komisen Pembuat ditetapkan oleh Penjual, atau cipta iterasi baru Blueprint ini dan sertakan ia sebagai sambungan dalam Blueprint anda sendiri untuk berkongsi hasil.

Perbincangan

(0)

Log masuk untuk menyertai perbincangan

Memuatkan komen...