Potassium Persulfate by Electrolysis of Potassium Bisulfate
Charlie

Dicipta oleh

Charlie

17. Oktober 2026DE
1
0
0
0
0

Potassium Persulfate by Electrolysis of Potassium Bisulfate

Potassium persulfate, the initiator that starts emulsion polymerisation (PVA glue), is made by electrolysing a cold, concentrated potassium bisulfate solution at about 1 A/dm² on a platinum anode with a graphite cathode. Sulfate is oxidised to persulfate at the anode, and the sparingly soluble salt crystallises out. It is a strong oxidant: keep it away from organic matter. The picture: our diagram of the cell.
Pertengahan
One to several days

Arahan

1

Make a strong, cold solution

Dissolve the potassium bisulfate in distilled water to a concentrated solution and keep it cold. A dilute solution gives oxygen instead of persulfate.

Bahan untuk langkah ini:

Kalium bisulfatKalium bisulfat400 g
Air SulingAir Suling1 liter

Alatan diperlukan:

Tangki elektrolisisTangki elektrolisis
Penimbang Dapur DigitalPenimbang Dapur Digital
TermometerTermometer
Sarung Tangan Kalis KimiaSarung Tangan Kalis Kimia
Cermin mata keselamatanCermin mata keselamatan
2

Electrolyse at high current density

Use a platinum anode and a graphite cathode. Run about 1 A per dm² of anode; hydrogen comes off at the cathode.

Alatan diperlukan:

Dawai platinumDawai platinum
Elektrod grafitElektrod grafit
Unit kuasa arus terusUnit kuasa arus terus
Tangki elektrolisisTangki elektrolisis
TermometerTermometer
3

Collect the crystals

Potassium persulfate crystallises out as it forms. Filter it off, rinse with a little cold distilled water and dry it (our method).

Alatan diperlukan:

Corong Büchner (porselin)Corong Büchner (porselin)
Kertas TurasKertas Turas
Dulang pengering terbukaDulang pengering terbuka
Sarung Tangan Kalis KimiaSarung Tangan Kalis Kimia
4

Use as initiator

For emulsion polymerisation, about 0.1–0.5 % is used, usually at 75–95 °C. Store it apart from organic materials.

Alatan diperlukan:

Penimbang Dapur DigitalPenimbang Dapur Digital
5

Charge and time

Memuatkan buku nota Jupyter…

Bahan

2
  • Pemegang Tempat
  • 1 liter
    Pemegang Tempat

Alatan Diperlukan

11

CC0 Domain Awam

Blueprint ini dikeluarkan di bawah CC0. Anda bebas menyalin, mengubah, mengedar, dan menggunakan karya ini untuk sebarang tujuan, tanpa meminta kebenaran.

Sokong Pembuat dengan membeli produk melalui Blueprint mereka di mana mereka memperoleh Komisen Pembuat ditetapkan oleh Penjual, atau cipta iterasi baru Blueprint ini dan sertakan ia sebagai sambungan dalam Blueprint anda sendiri untuk berkongsi hasil.

Perbincangan

(0)

Log masuk untuk menyertai perbincangan

Memuatkan komen...