Precipitated Silica: Hot Water Glass Carbonated, Then Acidified to pH 6.75 (Allen 1957)
Bubble carbon dioxide through hot dilute water glass and the silica comes down as an extremely fine white powder rather than a gel. Edward Allen of Columbia-Southern made it this way as a white reinforcing filler for rubber; this follows his Example XI, which gave a powder of 148 m² per gram.
Source: E. M. Allen (Columbia-Southern), US 2,805,955 (1957), Example XI. The percentages are our arithmetic; the filter, mill and indicator are ours. Picture drawn by Youblob.
Pertengahan
2 days
Arahan
1
1
Dilute the water glass
Dilute the water glass
Take 12,850 g of sodium silicate solution holding 976 g Na2O and 3115 g SiO2 (7.6 % and 24.2 %, a silica to soda ratio of 3.19 by weight; our arithmetic). Dilute it with water to 48 litres in a stirred kettle with a heating coil and thermometer, and heat to 95 °C.
Bahan untuk langkah ini:
Kaca air (larutan natrium silikat)12850 g
Air1 as requiredAlatan diperlukan:
Reaktor bertekanan
Pengacau
Termometer
Neraca dua piring2
2
Carbonate for an hour
Carbonate for an hour
Bubble in pure carbon dioxide fast enough to add the theoretical amount in about 30 minutes, and keep going at that rate for about 1 hour. The slurry ends at pH 9.85.
Alatan diperlukan:
Gas karbon dioksida
Reaktor bertekanan
Pengacau
Termometer
Kertas penunjuk pH3
3
Filter and wash
Filter and wash
Filter the slurry and wash the cake twice with hot water.
Bahan untuk langkah ini:
Air1 as requiredAlatan diperlukan:
Corong Büchner (porselin)
Kertas Turas4
4
Acidify to pH 6.75
Acidify to pH 6.75
Stir the cake back into water and bring it to pH 6.75 with 400 ml of 3.5 N hydrochloric acid.
Bahan untuk langkah ini:
Air1 as requiredAlatan diperlukan:
Asid hidroklorik
Bekas kaca
Pengacau
Kertas penunjuk pH5
5
Wash out the chloride
Wash out the chloride
Filter again and wash the cake with hot water until it is nearly free of chloride.
Bahan untuk langkah ini:
Air1 as requiredAlatan diperlukan:
Corong Büchner (porselin)
Kertas Turas6
6
Dry at 105 °C and grind
Dry at 105 °C and grind
Dry it at 105 °C in a fan oven and grind it to a fine powder. Allen's had a pH of 8.2, 0.61 % sodium and a surface area of 148 m² per gram.
Alatan diperlukan:
Ketuhar pengeringan
Lesung dan Alu
Balang Kaca BertutupBahan
2- Pemegang Tempat
- 4 as requiredPemegang Tempat
Alatan Diperlukan
13- Pemegang Tempat
- Pemegang Tempat
- Pemegang Tempat
- Pemegang Tempat
- Pemegang Tempat
- Pemegang Tempat
- Pemegang Tempat
- Pemegang Tempat
- Pemegang Tempat
- Pemegang Tempat
- Pemegang Tempat
- Pemegang Tempat
- Pemegang Tempat
Blueprint ini membuat
Blueprint berkaitan
Blueprint ini berkongsi pengetahuan — teknik, bahan atau prinsip
CC0 Domain Awam
Blueprint ini dikeluarkan di bawah CC0. Anda bebas menyalin, mengubah, mengedar, dan menggunakan karya ini untuk sebarang tujuan, tanpa meminta kebenaran.
Sokong Pembuat dengan membeli produk melalui Blueprint mereka di mana mereka memperoleh Komisen Pembuat ditetapkan oleh Penjual, atau cipta iterasi baru Blueprint ini dan sertakan ia sebagai sambungan dalam Blueprint anda sendiri untuk berkongsi hasil.