PTFE Fine Powder: a Dispersion Stirred Until It Curdles (Lontz 1952)
Charlie

Dicipta oleh

Charlie

28. Oktober 2026DE
13
0
0
0
0

PTFE Fine Powder: a Dispersion Stirred Until It Curdles (Lontz 1952)

A PTFE dispersion is stable on the shelf, but stirred hard enough it curdles. Fifty seconds at 1000 rpm in a baffled beaker and the polymer floats up as a dry-looking, unwettable crumb. Washed and dried, it is a free-flowing powder for rolling into tape, or for cold lubricated extrusion. Source: J. F. Lontz (du Pont), US 2,593,583 (1952), Example 1. Lontz started from a dispersion made with disuccinic acid peroxide; ours is Berry's persulfate dispersion, diluted to his 17 %. Picture drawn by Youblob.
Pertengahan
1 day

Arahan

1

Dilute the dispersion to 17 %

Ours: stir the 34 % dispersion with an equal weight of distilled water to get 17 % solids, the strength Lontz used.

Bahan untuk langkah ini:

Serakan PTFE berairSerakan PTFE berair1 part
Air SulingAir Suling1 part

Alatan diperlukan:

Neraca dua piringNeraca dua piring
Balang Kaca BertutupBalang Kaca Bertutup
2

Set up the baffled beaker

A 1-gallon stainless beaker, 6.5 in across and 7.5 in deep, with four baffles about ⅜ × 1 in hanging from the cover to within 3 in of the bottom. Stirrer: open turbine, 4 blades 1½ in high, 5 in across, reaching to within 1 in of the bottom.

Alatan diperlukan:

Tangki pengaduk bersekatTangki pengaduk bersekat
PengacauPengacau
3

Stir hard at 176 °F for 50 seconds

Put in half a gallon of the 17 % dispersion and heat it to 176 °F (80 °C). Run the stirrer at 1000 rpm for 50 seconds (Lontz measured 0.72 hp per gallon). The polymer coagulates and floats, unwetted, on top.

Alatan diperlukan:

Tangki pengaduk bersekatTangki pengaduk bersekat
PengacauPengacau
Plat PemanasPlat Pemanas
TermometerTermometer
4

Wash hot, then cold

Pour off the water. Wash the polymer with hot water at 176 °F, then with cold water at 60 °F (16 °C), and drain.

Alatan diperlukan:

Tangki pengaduk bersekatTangki pengaduk bersekat
TermometerTermometer
5

Dry at 230 °F for 16 hours

Spread the wet polymer on a 100-mesh screen and dry it in an oven at 230 °F (110 °C) for 16 hours. It comes out a free-flowing granular powder that passes 6–8 mesh.

Alatan diperlukan:

Ayak dawai halusAyak dawai halus
Ketuhar pengeringanKetuhar pengeringan
Balang Kaca BertutupBalang Kaca Bertutup

Bahan

2

Alatan Diperlukan

8

Blueprint berkaitan

Blueprint ini berkongsi pengetahuan — teknik, bahan atau prinsip

CC0 Domain Awam

Blueprint ini dikeluarkan di bawah CC0. Anda bebas menyalin, mengubah, mengedar, dan menggunakan karya ini untuk sebarang tujuan, tanpa meminta kebenaran.

Sokong Pembuat dengan membeli produk melalui Blueprint mereka di mana mereka memperoleh Komisen Pembuat ditetapkan oleh Penjual, atau cipta iterasi baru Blueprint ini dan sertakan ia sebagai sambungan dalam Blueprint anda sendiri untuk berkongsi hasil.