PTFE Rod: a Plug Sintered in Boiling Retene Vapour (Brubaker & Hanford 1946)
Emma

Dicipta oleh

Emma

27. Oktober 2026SE
12
0
0
0
0

PTFE Rod: a Plug Sintered in Boiling Retene Vapour (Brubaker & Hanford 1946)

The first example of du Pont's way to shape PTFE: press a small rod of powder cold, then heat it above 327 °C out of the mould. Here the heat comes from the vapour of boiling retene, which boils at 394 °C, so the temperature holds steady by itself. The plug comes out sintered into one tough piece. Source: M. M. Brubaker and W. E. Hanford (du Pont), US 2,400,099 (1946), Example I. The pressure is the patent's usual range, as the example gives none. The mould, press and the vapour-bath set-up are ours. Picture drawn by Youblob.
Lanjutan
1 day

Arahan

1

Press a plug from the powder

At room temperature, press small particles of PTFE in a mould into a plug 0.5 in across and 0.7 in long. The example gives no pressure; the patent's usual range is 100–3000 lb/sq in.

Bahan untuk langkah ini:

Serbuk resin PTFESerbuk resin PTFE1 as required for the plug

Alatan diperlukan:

Acuan mampatanAcuan mampatan
Mesin tekan hidraulikMesin tekan hidraulik
PembarisPembaris
2

Set up a retene vapour bath

Boil retene so its vapour fills the space round a glass tube. Ours: retene in a flask on a burner, a reflux condenser on top, and the tube standing in the vapour.

Alatan diperlukan:

RetenaRetena
Kelalang Penyulingan KacaKelalang Penyulingan Kaca
Kondenser RefluksKondenser Refluks
Penunu BunsenPenunu Bunsen
Tabung ujiTabung uji
3

Sinter for 3 hours

Take the plug out of the mould, put it in the glass tube, and heat it in the vapour of boiling retene (394 °C) for 3 hours.

Alatan diperlukan:

Tabung ujiTabung uji
RetenaRetena
Penunu BunsenPenunu Bunsen
4

Cool it under the retene

Remove the heat source and let the plug cool where it is. It is now sintered together into a tough mass.

Alatan diperlukan:

Tabung ujiTabung uji

Bahan

1
  • 1 as required for the plug
    Pemegang Tempat

Alatan Diperlukan

8

Blueprint ini membuat

CC0 Domain Awam

Blueprint ini dikeluarkan di bawah CC0. Anda bebas menyalin, mengubah, mengedar, dan menggunakan karya ini untuk sebarang tujuan, tanpa meminta kebenaran.

Sokong Pembuat dengan membeli produk melalui Blueprint mereka di mana mereka memperoleh Komisen Pembuat ditetapkan oleh Penjual, atau cipta iterasi baru Blueprint ini dan sertakan ia sebagai sambungan dalam Blueprint anda sendiri untuk berkongsi hasil.

Perbincangan

(0)

Log masuk untuk menyertai perbincangan

Memuatkan komen...