PTFE Thread Seal Tape: Paste-Extruded, Calendered, Never Sintered
Emma

Dicipta oleh

Emma

26. Oktober 2026SE
12
0
0
0
0

PTFE Thread Seal Tape: Paste-Extruded, Calendered, Never Sintered

The white tape wound on pipe threads is PTFE that has never been melted. Fine PTFE powder is mixed with a lubricant, pressed into a slug, squeezed through a slit die by a ram, rolled thin between two rolls, and dried. Kept below the sintering heat (about 350 °C) it stays soft and conforms to the thread (process: US 5,415,939, 1995). The targets and tests are those of the Indian standard IS 14643 (from BS 4375): no fillers, at most 0.1 % lubricant left, usually 12 mm wide and 0.075 mm thick. The lubricant (naphtha) and the slitter are ours. The picture: Fig. 1a of the patent.
Lanjutan
1 day

Arahan

1

Wet the powder

Mix fine (dispersion-made) virgin PTFE powder with a lubricant that can be driven off completely. Granular PTFE will not paste-extrude. No fillers. Ours: naphtha, as required.

Bahan untuk langkah ini:

Serbuk halus PTFESerbuk halus PTFE1 batch

Alatan diperlukan:

NaftaNafta
2

Press a preform

Compact the wet powder into a cylindrical preform in a mould with a plunger.

Alatan diperlukan:

Acuan mampatanAcuan mampatan
Mesin tekan hidraulikMesin tekan hidraulik
3

Ram-extrude a flat tape

Put the preform in the extrusion press. The plunger pushes it out through a slit die as a thick flat tape.

Alatan diperlukan:

Mesin penekan semperitan hidraulikMesin penekan semperitan hidraulik
4

Calender it thin

Pass the tape between two counter-rotating rolls to a thin tape, aiming at about 0.075 mm.

Alatan diperlukan:

Kilang gelek logamKilang gelek logam
MikrometerMikrometer
5

Dry off the lubricant

Dry the tape until the lubricant is gone. Keep it well below the sintering heat (about 350 °C): sintered tape is stiff and will not seal.

Alatan diperlukan:

Ketuhar pengeringanKetuhar pengeringan
6

Slit and spool

Slit it to width, usually 12 mm (±0.5 mm), and wind it on spools.

Alatan diperlukan:

Mesin belah-gulung semulaMesin belah-gulung semula
7

Check the tape

It must look white, with no visible specks or torn edges. Measure the thickness at five points along a sample; each must be within 10 % of their mean.

Alatan diperlukan:

MikrometerMikrometer
8

Test the residual lubricant

Weigh about 15 g of tape. Extract it in a Soxhlet with petroleum spirit (40-60 °C) for at least 4 h, dry it at 100 °C, then heat it at 300 °C for 6 h, cool and weigh. The loss must be 0.1 % or less.

Alatan diperlukan:

Pengekstrak SoxhletPengekstrak Soxhlet
Eter petroleumEter petroleum
Ketuhar pengeringanKetuhar pengeringan
Mangkuk pijar keluliMangkuk pijar keluli
Kebuk pengeringan (kecil)Kebuk pengeringan (kecil)
Penimbang Digital JituPenimbang Digital Jitu
9

Wrap a thread

Wind tape round an R 1/2 taper pipe thread with 50 % overlap, two layers deep, just tight enough to take the thread form. It must hold the form, not break, and its end must stay put.

Alatan diperlukan:

Penyambung paip berbenangPenyambung paip berbenang

Bahan

1

Alatan Diperlukan

14

CC0 Domain Awam

Blueprint ini dikeluarkan di bawah CC0. Anda bebas menyalin, mengubah, mengedar, dan menggunakan karya ini untuk sebarang tujuan, tanpa meminta kebenaran.

Sokong Pembuat dengan membeli produk melalui Blueprint mereka di mana mereka memperoleh Komisen Pembuat ditetapkan oleh Penjual, atau cipta iterasi baru Blueprint ini dan sertakan ia sebagai sambungan dalam Blueprint anda sendiri untuk berkongsi hasil.

Perbincangan

(0)

Log masuk untuk menyertai perbincangan

Memuatkan komen...