Saw File: Three-Square, Forged in a Boss, Cut by Hand and Hardened (Ure, 1839)
Forge

Dicipta oleh

Forge

4. November 2026NO
12
0
0
0
0

Saw File: Three-Square, Forged in a Boss, Cut by Hand and Hardened (Ure, 1839)

The file for sharpening saw teeth as Sheffield made it by hand: a three-square (triangular) bar of cast steel, not tapering, forged in a V-shaped boss, its teeth cut one by one with a chisel and hammer, then hardened under a coat of animal carbon and salt and quenched in cold spring water. Ure says saw files in particular should be hardened with the carbon mixture, so they will cut iron and steel. Not given: sizes and teeth per inch. Source: A. Ure, Dictionary of Arts, Manufactures, and Mines (1839), File. Picture: our drawing.
Lanjutan
Unknown

Arahan

1

Forge the blank

Draw cast steel out square at the forge, then lay it with one angle down in a boss whose recess has two sides meeting at an angle, so the hammer forms one side and the boss the other two. Keep it the same size along its length (saw files are not tapered).

Bahan untuk langkah ini:

Keluli mangkuk pijarKeluli mangkuk pijar1 cast steel bar
Dimensi tidak diketahuiDimensi tidak diketahui1 keping

Alatan diperlukan:

Relau tukang besiRelau tukang besi
Penyepit Tukang BesiPenyepit Tukang Besi
Swage bawahSwage bawah
TukulTukul
Tukul besarTukul besar
2

Cut the teeth

On an anvil with a flat, even face, hold the file down with a leather strap over each end, the workman's feet in the straps like stirrups. Cut the teeth with a chisel a little broader than the file, sharpened to about 20 degrees, struck with a hammer of 1 to 6 lb. For single cut, run a fine file lightly over the teeth to take off the roughness; for double cut, cut a second set nearly at right angles to the first.

Alatan diperlukan:

Andas keluliAndas keluli
Tali KulitTali Kulit
Pahat besi sejukPahat besi sejuk
TukulTukul
Kikir LogamKikir Logam
3

Cut the other sides

To cut the next side, lay the file in a piece of lead-tin alloy with an angular groove, so the teeth already cut are not spoiled on the anvil.

Alatan diperlukan:

Pateri timah-plumbumPateri timah-plumbum
Andas keluliAndas keluli
Pahat besi sejukPahat besi sejuk
TukulTukul
4

Coat for hardening

Distil shoemakers' and curriers' leather refuse in an iron still and powder the bright coal left. Grind about equal parts by bulk of this carbon and salt to the consistence of cream with water and cover the file with it.

Alatan diperlukan:

Retort besiRetort besi
GaramGaram
AirAir
5

Harden

Hold the file by the tang in a fire of very small cokes, drawing it out often, until it is an even cherry red from tang to point. Plunge it straight down, quickly, into clear spring water as cold as possible.

Alatan diperlukan:

Relau tukang besiRelau tukang besi
Kok metalurgiKok metalurgi
Penyepit Tukang BesiPenyepit Tukang Besi
AirAir
6

Clean and oil

Brush the file with water and powdered cokes until clean and metallic, wash it in two or three waters to take off all the salt, dip it in lime-water, dry it quickly before the fire and oil it while warm with olive oil containing a little oil of turpentine.

Alatan diperlukan:

Kok metalurgiKok metalurgi
AirAir
Air kapurAir kapur
Minyak zaitunMinyak zaitun
TurpentinTurpentin

Bahan

2

Alatan Diperlukan

17

CC0 Domain Awam

Blueprint ini dikeluarkan di bawah CC0. Anda bebas menyalin, mengubah, mengedar, dan menggunakan karya ini untuk sebarang tujuan, tanpa meminta kebenaran.

Sokong Pembuat dengan membeli produk melalui Blueprint mereka di mana mereka memperoleh Komisen Pembuat ditetapkan oleh Penjual, atau cipta iterasi baru Blueprint ini dan sertakan ia sebagai sambungan dalam Blueprint anda sendiri untuk berkongsi hasil.

Perbincangan

(0)

Log masuk untuk menyertai perbincangan

Memuatkan komen...