Neodymium Magnets, Sample 21: 75Fe-8B-17Nd Sintered (Sagawa 1988)
Neodymium magnets are iron, boron and neodymium. Sagawa's team at Sumitomo melted the three together, ground the casting to a powder finer than 10 µm, lined the grains up in a magnetic field while pressing them, and sintered the compact in argon. This is their sample 21, 75 % iron, 8 % boron and 17 % neodymium by atoms: 31.1 MGOe.
Source: M. Sagawa et al. (Sumitomo Special Metals), US 4,770,723 (1988). Unknown: how the pure iron, the ferroboron and the neodymium metal are made; the patent does not say. The magnetising is ours, after Przybylski et al., Sensors 16:569 (2016). The 1 kg weights are our arithmetic from the patent's atomic percentages. Picture: the patent's Fig. 8.
Pakar
2 days
Arahan
1
1
Weigh sample 21: 75 Fe, 8 B, 17 Nd
Weigh sample 21: 75 Fe, 8 B, 17 Nd
Sample 21 is 75 % iron, 8 % boron and 17 % neodymium by atoms. Use 99.9 % electrolytic iron, ferroboron (19.38 % B, 5.32 % Al, 0.74 % Si, 0.03 % C, the rest iron) and neodymium of 99.7 % or better. Ours: a 1 kg melt, by arithmetic: 573.2 g iron, 66.3 g ferroboron, 364.5 g neodymium. Unknown: how these three are made.
Bahan untuk langkah ini:
Besi elektrolitik573.2 g
Ferroboron66.3 g
Logam neodimium364.5 gAlatan diperlukan:
Neraca dua piring2
2
Melt by high frequency in argon and cast
Melt by high frequency in argon and cast
Melt the charge in a high-frequency (induction) furnace under argon and pour it into a water-cooled copper mould.
Alatan diperlukan:
Relau aruhan
Mangkuk Pijar Tanah Liat Tahan Api
Argon
Silinder gas bertekanan
Acuan kuprum disejukkan air
Sarung Tangan Tahan Haba3
3
Stamp to 35 mesh, ball-mill to 3-10 µm
Stamp to 35 mesh, ball-mill to 3-10 µm
Crush the casting in a stamp mill until it passes a 35-mesh sieve. Then grind it in a ball mill for 3 hours, to 3-10 µm.
Alatan diperlukan:
Kilang Penumbuk
Set penapis (mata bergred)
Kilang Bebola Besi
Cermin mata keselamatan4
4
Press in a 10 kOe field at 1.5 t/cm²
Press in a 10 kOe field at 1.5 t/cm²
Line the powder up in a magnetic field of 10 kOe and press it at 1.5 tonnes per cm². Unknown: the size and shape of the magnets.
Alatan diperlukan:
Penekan medan magnet5
5
Sinter in argon at 1000-1200 °C
Sinter in argon at 1000-1200 °C
Sinter the compacts at 1000-1200 °C for about one hour in argon, then let them cool. Sample 21 measured 11.6 kG remanence, 9.2 kOe coercivity and 31.1 MGOe.
Alatan diperlukan:
Relau Tiub
Argon
Silinder gas bertekanan
Sarung Tangan Tahan Haba6
6
Magnetise the magnets
Magnetise the magnets
Ours, after Przybylski et al., Sensors 16:569 (2016): put each magnet in the coil of an impulse magnetiser and discharge a capacitor bank through it. They found a field of 1200 kA/m enough to saturate N38 sintered Nd-Fe-B; their magnetiser used a 1 mF bank charged up to 5000 V, a thyristor switch and a 440-turn coil of 3 mm copper wire with an 80 mm bore.
Alatan diperlukan:
PemagnetBahan
3- 573.2 gPemegang Tempat
- 66.3 gPemegang Tempat
- 364.5 gPemegang Tempat
Alatan Diperlukan
14- Pemegang Tempat
- Pemegang Tempat
- Pemegang Tempat
- Pemegang Tempat
- Pemegang Tempat
- Pemegang Tempat
- Pemegang Tempat
- Pemegang Tempat
- Pemegang Tempat
- Pemegang Tempat
- Pemegang Tempat
- Pemegang Tempat
- Pemegang Tempat
- Pemegang Tempat
Blueprint ini membuat
Blueprint berkaitan
Blueprint ini berkongsi pengetahuan — teknik, bahan atau prinsip
CC0 Domain Awam
Blueprint ini dikeluarkan di bawah CC0. Anda bebas menyalin, mengubah, mengedar, dan menggunakan karya ini untuk sebarang tujuan, tanpa meminta kebenaran.
Sokong Pembuat dengan membeli produk melalui Blueprint mereka di mana mereka memperoleh Komisen Pembuat ditetapkan oleh Penjual, atau cipta iterasi baru Blueprint ini dan sertakan ia sebagai sambungan dalam Blueprint anda sendiri untuk berkongsi hasil.