Anvil: Wrought-Iron Body with a Welded Steel Face
Forge

Dicipta oleh

Forge

11. Oktober 2026NO
40
0
0
0
0

Anvil: Wrought-Iron Body with a Welded Steel Face

Outside the United States, anvils of the 1880s had a body of wrought iron under a steel face, and a horn of plain wrought iron. The body was roughly shaped under tilt hammers, in one piece or with the corners and horn welded on. A face plate of shear or blister steel, 3/8 to 3/4 inch thick, was forge-welded to it a few inches at a time by four strikers, then the holes were punched and the anvil dressed to shape, ground flat and hardened under a falling stream of water. A well-welded anvil rings clearly when struck. Most modern anvils are instead cast steel with the face hardened by flame or induction.
Lanjutan
Works process (1880s)

Arahan

1

Shape the body

Rough out the wrought-iron body under the tilt hammer, in one piece or with the corners and horn welded on.

Bahan untuk langkah ini:

Bar besi tempaBar besi tempa1 as required

Alatan diperlukan:

Tukul jatuhTukul jatuh
Relau tukang besiRelau tukang besi
2

Weld on the face

Bring the body and the steel face plate to a welding heat and weld from one end, about five inches at a time with four strikers, heat after heat, until the whole face is on. Take care not to burn the steel.

Bahan untuk langkah ini:

Plat keluli shearPlat keluli shear1 keping

Alatan diperlukan:

Relau tukang besiRelau tukang besi
Tukul besarTukul besar
3

Punch and dress

Punch the hardy (cutter) hole and the small round hole in the tail, round the horn, and dress the anvil to shape at another heat.

Alatan diperlukan:

Penebuk panasPenebuk panas
Tukul besarTukul besar
4

Grind

Grind any unevenness out of the face, crosswise on a large stone.

Alatan diperlukan:

Batu canai rodaBatu canai roda
5

Harden

Reheat the top to a red heat and let a stream of water fall on it from a ten-foot head. A clear ring when struck shows a sound weld.

Bahan untuk langkah ini:

AirAir1 as required

Alatan diperlukan:

Relau tukang besiRelau tukang besi

Bahan

3
  • 1 as required
    Pemegang Tempat
  • Pemegang Tempat
  • 1 as required
    Pemegang Tempat

Alatan Diperlukan

5

Blueprint ini membuat

CC0 Domain Awam

Blueprint ini dikeluarkan di bawah CC0. Anda bebas menyalin, mengubah, mengedar, dan menggunakan karya ini untuk sebarang tujuan, tanpa meminta kebenaran.

Sokong Pembuat dengan membeli produk melalui Blueprint mereka di mana mereka memperoleh Komisen Pembuat ditetapkan oleh Penjual, atau cipta iterasi baru Blueprint ini dan sertakan ia sebagai sambungan dalam Blueprint anda sendiri untuk berkongsi hasil.

Perbincangan

(0)

Log masuk untuk menyertai perbincangan

Memuatkan komen...