Strontium-Calcium Ferrite Disc Magnet: 0.08 mol SrCO3 and 0.02 mol CaCO3, 1280 °C (Went, Philips 1956, Ex. 23)
Charlie

Dicipta oleh

Charlie

28. Oktober 2026DE
4
0
0
0
0

Strontium-Calcium Ferrite Disc Magnet: 0.08 mol SrCO3 and 0.02 mol CaCO3, 1280 °C (Went, Philips 1956, Ex. 23)

A strontium ferrite with a fifth of the strontium replaced by calcium: 0.08 mol strontium carbonate and 0.02 mol calcium carbonate to 0.6 mol iron oxide, ground, dried, formed and passed through a 1280 °C furnace in 10 minutes. Went's rod held 2,320 gauss with a coercive force of 1,395 oersted. Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 23. They sintered rods; discs and the magnetising are ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Lanjutan
2 days

Arahan

1

Weigh the carbonates and iron oxide

Weigh 11.81 g strontium carbonate (0.08 mol), 2.002 g calcium carbonate (0.02 mol), 95.55 g ferric oxide (0.6 mol).

Bahan untuk langkah ini:

Strontium karbonatStrontium karbonat11.81 g
Kalsium karbonat (kapur putih halus)Kalsium karbonat (kapur putih halus)2.002 g
Ferik OksidaFerik Oksida95.55 g

Alatan diperlukan:

Neraca dua piringNeraca dua piring
Alat Pernafasan P100Alat Pernafasan P100
2

Mill with alcohol 4 hours, dry

As in Examples 18 to 21: grind the mixture with alcohol in a ball mill for 4 hours, then dry it.

Alatan diperlukan:

Kilang Bebola BesiKilang Bebola Besi
Etanol mutu makmal, 95 %Etanol mutu makmal, 95 %
Ketuhar pengeringanKetuhar pengeringan
3

Press at 1.5 t/cm²

Example 23 does not say whether the 1000 °C presinter of Examples 18 to 21 is used. Press the dry powder at 1.5 tonnes per cm² (ours: discs instead of a rod).

Alatan diperlukan:

Mesin tekan hidraulikMesin tekan hidraulik
Acuan tekan cakeraAcuan tekan cakera
4

Pass through a 1280 °C zone in 10 minutes

Sinter at 1280 °C by passing the pieces through a 10 cm hot zone at 10 mm per minute: 10 minutes in the heat.

Alatan diperlukan:

Relau TiubRelau Tiub
Sarung Tangan Tahan HabaSarung Tangan Tahan Haba
5

Magnetise the discs

The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.

Alatan diperlukan:

ElektromagnetElektromagnet
KompasKompas

Bahan

3

Alatan Diperlukan

11

CC0 Domain Awam

Blueprint ini dikeluarkan di bawah CC0. Anda bebas menyalin, mengubah, mengedar, dan menggunakan karya ini untuk sebarang tujuan, tanpa meminta kebenaran.

Sokong Pembuat dengan membeli produk melalui Blueprint mereka di mana mereka memperoleh Komisen Pembuat ditetapkan oleh Penjual, atau cipta iterasi baru Blueprint ini dan sertakan ia sebagai sambungan dalam Blueprint anda sendiri untuk berkongsi hasil.

Perbincangan

(0)

Log masuk untuk menyertai perbincangan

Memuatkan komen...