Strontium-Calcium Ferrite Disc Magnet: 0.06 mol SrCO3 and 0.04 mol CaCO3, 1280 °C (Went, Philips 1956, Ex. 24)
A strontium ferrite with 0.06 mol strontium carbonate and 0.04 mol calcium carbonate to 0.6 mol iron oxide, made as in Example 23. Went's rod held 2,120 gauss with a coercive force of 1,950 oersted.
Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 24. They sintered rods; discs and the magnetising are ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Lanjutan
2 days
Arahan
1
1
Weigh the carbonates and iron oxide
Weigh the carbonates and iron oxide
Weigh 8.86 g strontium carbonate (0.06 mol), 4.004 g calcium carbonate (0.04 mol), 95.55 g ferric oxide (0.6 mol). The patent prints 81.86 g of strontium carbonate beside 0.06 mol. 0.06 mol is 8.86 g (ours, at 147.63 g per mol), the weight used here.
Bahan untuk langkah ini:
Strontium karbonat8.86 g
Kalsium karbonat (kapur putih halus)4.004 g
Ferik Oksida95.55 gAlatan diperlukan:
Neraca dua piring
Alat Pernafasan P1002
2
Mill with alcohol 4 hours, dry
Mill with alcohol 4 hours, dry
As in Example 23: grind the mixture with alcohol in a ball mill for 4 hours, then dry it.
Alatan diperlukan:
Kilang Bebola Besi
Etanol mutu makmal, 95 %
Ketuhar pengeringan3
3
Press at 1.5 t/cm²
Press at 1.5 t/cm²
Press the dry powder at 1.5 tonnes per cm² (ours: discs instead of a rod).
Alatan diperlukan:
Mesin tekan hidraulik
Acuan tekan cakera4
4
Pass through a 1280 °C zone in 10 minutes
Pass through a 1280 °C zone in 10 minutes
Sinter at 1280 °C by passing the pieces through a 10 cm hot zone at 10 mm per minute: 10 minutes in the heat.
Alatan diperlukan:
Relau Tiub
Sarung Tangan Tahan Haba5
5
Magnetise the discs
Magnetise the discs
The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.
Alatan diperlukan:
Elektromagnet
KompasBahan
3- 8.86 gPemegang Tempat
- Pemegang Tempat
- 95.55 gPemegang Tempat
Alatan Diperlukan
11- Pemegang Tempat
- Pemegang Tempat
- Pemegang Tempat
- Pemegang Tempat
- Pemegang Tempat
- Pemegang Tempat
- Pemegang Tempat
- Pemegang Tempat
- Pemegang Tempat
- Pemegang Tempat
- Pemegang Tempat
Blueprint ini membuat
Blueprint berkaitan
Blueprint ini berkongsi pengetahuan — teknik, bahan atau prinsip
CC0 Domain Awam
Blueprint ini dikeluarkan di bawah CC0. Anda bebas menyalin, mengubah, mengedar, dan menggunakan karya ini untuk sebarang tujuan, tanpa meminta kebenaran.
Sokong Pembuat dengan membeli produk melalui Blueprint mereka di mana mereka memperoleh Komisen Pembuat ditetapkan oleh Penjual, atau cipta iterasi baru Blueprint ini dan sertakan ia sebagai sambungan dalam Blueprint anda sendiri untuk berkongsi hasil.