Table Tennis Balls: Celluloid Halves Blown in an Out-of-Round Mould (Jaques 1935)
J. M. Jaques · Public domain (US patent)
Emma

Dicipta oleh

Emma

27. Oktober 2026SE
11
0
0
0
0

Table Tennis Balls: Celluloid Halves Blown in an Out-of-Round Mould (Jaques 1935)

A celluloid table tennis ball is two stamped halves sealed with acetone, then blown out round by its own air in a hot mould. The overlapped seam shrinks a little as it cools, so the ball ends slightly narrower across the seam. John Jaques made the mould wider across the seam by just that amount, so the ball cools truly round. Source: J. M. Jaques, US 2,025,455 (1935). The patent gives no sheet thickness, ball size or temperatures. The press, pot and micrometer are ours. Picture: the patent drawing.
Pertengahan
1 day

Arahan

1

Stamp two halves from hot sheet

Stamp two half-balls out of celluloid sheet while it is hot. The patent gives no temperature.

Bahan untuk langkah ini:

SeluloidSeluloid1 helaian

Alatan diperlukan:

Acuan tekan separa sferaAcuan tekan separa sfera
Mesin penekan tebukMesin penekan tebuk
2

Seal the halves with acetone

Wet the edges of both halves with acetone, fit them together with the edges overlapping and let them seal. You now have a closed rough ball with a seam round its middle.

Alatan diperlukan:

AsetonAseton
3

Measure the seam shrinkage

Blown balls come out narrower across the seam than across the poles: about one to two ten-thousandths of an inch on the celluloid balls Jaques measured. For your own celluloid, measure it on a test ball.

Alatan diperlukan:

MikrometerMikrometer
4

Use a mould wider at the seam

The split mould is not a true sphere. Measured in the plane where its two halves meet (diameter A), it is wider than at right angles to that plane (diameter B) by the amount the seam shrinks, and it has small vents to let air out.

Alatan diperlukan:

Acuan bola dua belahAcuan bola dua belah
MikrometerMikrometer
5

Set the ball seam to joint

Lay the rough ball in the mould with its seam exactly on the mould joint, and hold it there with a little petroleum jelly so it cannot move.

Alatan diperlukan:

Acuan bola dua belahAcuan bola dua belah
VaselinVaselin
6

Blow it out in hot water

Close the mould and put it in hot water. The air inside the ball expands and blows the ball out to fill the mould.

Alatan diperlukan:

Acuan bola dua belahAcuan bola dua belah
Periuk BesarPeriuk Besar
AirAir
7

Cool and take out

Let the mould cool, then open it and take the ball out. As the seam shrinks it comes back to the same diameter as the rest, so the ball is as near round as it can be.

Alatan diperlukan:

Acuan bola dua belahAcuan bola dua belah

Bahan

1
  • 1 helaian
    Pemegang Tempat

Alatan Diperlukan

8

CC0 Domain Awam

Blueprint ini dikeluarkan di bawah CC0. Anda bebas menyalin, mengubah, mengedar, dan menggunakan karya ini untuk sebarang tujuan, tanpa meminta kebenaran.

Sokong Pembuat dengan membeli produk melalui Blueprint mereka di mana mereka memperoleh Komisen Pembuat ditetapkan oleh Penjual, atau cipta iterasi baru Blueprint ini dan sertakan ia sebagai sambungan dalam Blueprint anda sendiri untuk berkongsi hasil.

Perbincangan

(0)

Log masuk untuk menyertai perbincangan

Memuatkan komen...