Terephthalic Acid: Para-Xylene Oxidised by Air with Manganese and Bromide
Charlie

Dicipta oleh

Charlie

19. Oktober 2026DE
7
0
0
0
0

Terephthalic Acid: Para-Xylene Oxidised by Air with Manganese and Bromide

Terephthalic acid is the acid half of PET. Both methyl groups of para-xylene are burnt to acid groups by air under pressure in hot acetic acid, with a little manganese salt and bromide as catalyst: the Mid-Century process of Saffer and Barker (US 2,833,816, 1958). The acid does not dissolve, so it is simply filtered off. Example 24 of the patent, all parts by weight. The picture: our diagram of the reactor.
Lanjutan
1 day

Arahan

1

Charge the reactor

Into a corrosion-resistant pressure reactor with a water-cooled condenser on top, put 75 parts para-xylene, 150 parts acetic acid, 1 part manganese acetate (tetrahydrate) and 0.75 part ammonium bromide.

Bahan untuk langkah ini:

Para-xilenaPara-xilena75 parts

Alatan diperlukan:

Asid asetik (glasier)Asid asetik (glasier)
Mangan AsetatMangan Asetat
Ammonium BromidaAmmonium Bromida
Neraca dua piringNeraca dua piring
Reaktor bertekananReaktor bertekanan
Gegelung kondenserGegelung kondenser
Gogal Percikan KimiaGogal Percikan Kimia
Sarung Tangan Kalis KimiaSarung Tangan Kalis Kimia
2

Pressurise with air and heat to 385 °F

Raise the pressure to 400 psig with air, blown in near the bottom. Set the vent so gas leaves at 3,000 volumes per hour per volume of liquid. Heat to 385 °F (196 °C), then switch the heat off: the reaction heats itself.

Alatan diperlukan:

Reaktor bertekananReaktor bertekanan
Pemampat udara industriPemampat udara industri
Gegelung kondenserGegelung kondenser
Termometer MakmalTermometer Makmal
3

Hold at 385–400 °F

Once the first rush is over, heat as needed to hold 385–400 °F (196–204 °C), 1.5 hours in all. It is finished when the exit gas is back to 20–21 % oxygen (Orsat analysis).

Alatan diperlukan:

Reaktor bertekananReaktor bertekanan
Termometer MakmalTermometer Makmal
Penganalisis Gas OrsatPenganalisis Gas Orsat
4

Cool, empty and filter

Cool to 185 °F (85 °C) and let the pressure off. Push the liquid out at 150–200 °F with nitrogen pressure, scrape out the solid, and filter everything together.

Alatan diperlukan:

Silinder Gas NitrogenSilinder Gas Nitrogen
Corong Kaca BertangkaiCorong Kaca Bertangkai
Kertas TurasKertas Turas
Sarung Tangan Kalis KimiaSarung Tangan Kalis Kimia
5

Wash and dry

Wash the terephthalic acid twice with hot acetic acid (75 ml each in the example) and dry it. The patent got 115 parts by weight from 100 of para-xylene.

Alatan diperlukan:

Asid asetik (glasier)Asid asetik (glasier)
Corong Kaca BertangkaiCorong Kaca Bertangkai
Kertas TurasKertas Turas
Ketuhar pengeringanKetuhar pengeringan

Bahan

1
  • 75 parts
    Pemegang Tempat

Alatan Diperlukan

15

Blueprint berkaitan

Blueprint ini berkongsi pengetahuan — teknik, bahan atau prinsip

CC0 Domain Awam

Blueprint ini dikeluarkan di bawah CC0. Anda bebas menyalin, mengubah, mengedar, dan menggunakan karya ini untuk sebarang tujuan, tanpa meminta kebenaran.

Sokong Pembuat dengan membeli produk melalui Blueprint mereka di mana mereka memperoleh Komisen Pembuat ditetapkan oleh Penjual, atau cipta iterasi baru Blueprint ini dan sertakan ia sebagai sambungan dalam Blueprint anda sendiri untuk berkongsi hasil.

Perbincangan

(0)

Log masuk untuk menyertai perbincangan

Memuatkan komen...