Violet Iron Oxide: Precipitated Hematite Calcined at 1000-1100 °C (Nurdini et al. 2022)
Charlie

Dicipta oleh

Charlie

1. November 2026DE
8
0
0
0
0

Violet Iron Oxide: Precipitated Hematite Calcined at 1000-1100 °C (Nurdini et al. 2022)

Iron hydroxide is thrown down from hot ferric nitrate solution with ammonia, washed, dried and calcined. All of it ends as pure hematite, but the colour moves from bright red through dark red to purple as the calcining heat rises from 1000 °C, because the grains grow larger and more crystalline. Result: pure violet to purple ferric oxide (hematite) after 4 hours at 1000-1100 °C. Source: Nurdini et al., Heliyon 8 (2022) e10377, sections 2.2 and 4. Not given: batch size, how much ammonia, end pH, yield. Picture drawn by Youblob.
Pertengahan
2 days

Arahan

1

Heat the ferric nitrate solution

Make a 0.05 M solution of ferric nitrate in distilled water and heat it to 80 °C.

Bahan untuk langkah ini:

Ferik NitratFerik Nitrat1 as required

Alatan diperlukan:

Air SulingAir Suling
Bikar KacaBikar Kaca
Plat PemanasPlat Pemanas
TermometerTermometer
2

Throw down the hydroxide with ammonia

Keeping it at 80 °C, add ammonia solution drop by drop while stirring well. Stir for 3 hours, then let it cool to room temperature: a red-brown precipitate forms. Not given: how much ammonia.

Alatan diperlukan:

Larutan ammonia 25-28 %Larutan ammonia 25-28 %
Corong TitisCorong Titis
Plat PemanasPlat Pemanas
TermometerTermometer
3

Spin down, wash and dry

Collect the precipitate in a centrifuge at 4000 rpm for 15 minutes, wash it with distilled water, and dry it at 110 °C for 24 hours.

Alatan diperlukan:

Emparan mejaEmparan meja
Air SulingAir Suling
Ketuhar pengeringanKetuhar pengeringan
4

Calcine at 1000-1100 °C

Calcine for 4 hours in air at 1000-1100 °C. Below 1000 °C it stays bright or dark red; from 1000 °C it turns purple. Grind the cooled oxide to a fine powder (they used an agate mortar).

Alatan diperlukan:

Relau MuffleRelau Muffle
Lesung dan AluLesung dan Alu

Bahan

1
  • 1 as required
    Pemegang Tempat

Alatan Diperlukan

10

CC0 Domain Awam

Blueprint ini dikeluarkan di bawah CC0. Anda bebas menyalin, mengubah, mengedar, dan menggunakan karya ini untuk sebarang tujuan, tanpa meminta kebenaran.

Sokong Pembuat dengan membeli produk melalui Blueprint mereka di mana mereka memperoleh Komisen Pembuat ditetapkan oleh Penjual, atau cipta iterasi baru Blueprint ini dan sertakan ia sebagai sambungan dalam Blueprint anda sendiri untuk berkongsi hasil.

Perbincangan

(0)

Log masuk untuk menyertai perbincangan

Memuatkan komen...