Fuller, Pritchel and Hot Setts: Steel Welded into a Split Iron Bar, with Twisted Rod or Withy Handles (Edwinson, 1886)
The smith's own top and bottom tools, from George Edwinson's farrier's chapter in Amateur Work (1886): an inch iron bar upset, split into a fork and a steel wedge welded in, then forged into a fuller, pritchel punch, curved or straight hot sett, or a square-tanged bottom sett; the pritchel itself from 1/2 in. square tool steel; handles of twisted iron rod or green withy.
Ilọsíwájú
A day at the forge for the set
Ìlànà
1
1
His proportions
His proportions
Ń ṣí ìwé Jupyter…
2
2
Read Edwinson
Read Edwinson
"To make this tool, heat and upset the end of an inch bar of iron; then heat again and split with a sett."
3
3
Split the iron
Split the iron
Heat and upset the end of a 1 in. (25 mm) iron bar. Heat again and split it with a hot set into a fork 1 to 1 1/4 in. long by 3/4 in. wide (his fig. 108).
Àwọn ohun èlò fún ìgbésẹ̀ yìí:
Ọ̀pá irin lílù1 ẹyọÀwọn irinṣẹ́ tí a nílò:
Ìléru alágbẹ̀dẹ
Ìdí Alágbẹ̀dẹ
Òòlù ńlá
Ìlù gbígbóná
Ẹmú alágbẹ̀dẹ4
4
Weld in the steel
Weld in the steel
Heat the end of a steel bar of similar size and forge a wedge to fit the fork (fig. 109). Bring both to a welding heat and weld them well together.
Àwọn ohun èlò fún ìgbésẹ̀ yìí:
Irin líle tí a yọ́ nínú ìkòkò1 ẹyọ
Erùpẹ̀ boraksi1 ẹyọÀwọn irinṣẹ́ tí a nílò:
Ìléru alágbẹ̀dẹ
Ìdí Alágbẹ̀dẹ
Òòlù ńlá
Ẹmú alágbẹ̀dẹ5
5
Forge the fuller
Forge the fuller
Cut off 2 in. of steel and 3 in. of iron for the tool. Forge the steel, with the iron behind it, into the fuller's rounded blade (fig. 102). Make the neck while it is still on the bar, then cut it off leaving a piece of iron for the head.
Àwọn irinṣẹ́ tí a nílò:
Ìléru alágbẹ̀dẹ
Ìdí Alágbẹ̀dẹ
Òòlù
Ìlù gbígbóná6
6
Same blank, other tools
Same blank, other tools
Pritchel punch: about 2 in. of iron and 1 in. of steel, shaped as fig. 103. Curved set: as the fuller but with a gouge-shaped blade (fig. 105). Top hot set: the same, with a chisel or wedge blade (fig. 106). Bottom set: a wedge of steel and iron, edge up, on a square tang that fits the anvil's square hole (fig. 107).
Àwọn ohun èlò fún ìgbésẹ̀ yìí:
Ọ̀pá irin lílù1 ẹyọ
Irin líle tí a yọ́ nínú ìkòkò1 ẹyọ
Erùpẹ̀ boraksi1 ẹyọÀwọn irinṣẹ́ tí a nílò:
Ìléru alágbẹ̀dẹ
Ìdí Alágbẹ̀dẹ
Òòlù
Òòlù ńlá
Ẹmú alágbẹ̀dẹ7
7
Forge the pritchel
Forge the pritchel
Forge 1/2 in. (13 mm) square tool steel into the tapered pritchel (fig. 104), 6 in. (150 mm) long. It punches nail holes in hot iron, so it need not be hardened.
Àwọn ohun èlò fún ìgbésẹ̀ yìí:
Ọ̀pá irin ohun èlò1 ẹyọÀwọn irinṣẹ́ tí a nílò:
Ìléru alágbẹ̀dẹ
Ìdí Alágbẹ̀dẹ
Òòlù
Ẹmú alágbẹ̀dẹ8
8
Fit the handles
Fit the handles
Rod handle: twist 3/8 in. iron rod once round the neck and weld the two ends together (fig. 110). Withy handle: take a green or half-green hazel, willow, oak or withy rod about 3 ft long, twist the middle 8-9 in., wrap it once round the neck and bind the two ends with wire or a link (figs. 106, 111).
Àwọn ohun èlò fún ìgbésẹ̀ yìí:
Ọ̀pá rírọ irin rírọ̀1 ẹyọ
Ẹ̀ka willow (tí ń tẹ̀)1 ẹyọ
Wáyà irin1 ẹyọÀwọn irinṣẹ́ tí a nílò:
Ìléru alágbẹ̀dẹ
Ìdí Alágbẹ̀dẹ
Òòlù
Ẹmú alágbẹ̀dẹ9
9
Harden the cutting tools (ours)
Harden the cutting tools (ours)
He gives no temper for these. Ours: harden and temper the set edges as for other hot-cutting tools, and cool them often in use.
Àwọn irinṣẹ́ tí a nílò:
Ìléru alágbẹ̀dẹ
Àpótí ìtutù10
10
Troubleshooting
Troubleshooting
Top-tool troubleshooting.
Flow
Loading...
11
11
History and honest limits
History and honest limits
From George Edwinson, "Smithing and Forging" VII, **Amateur Work, Illustrated**, vol. VI (1886-87), pp. 14-16 and figs. 101-111 (checked on the archive.org scan amateurworkillus06lond). He calls the top hot cutter a "sett"; we map it to the Hot Chisel head and the bottom sett to the Hot Cut Hardy head. Temper, metric figures and tools are ours.
Àwọn ohun-èlò
7- 1 ẹyọÀyè
- Àyè
- 1 ẹyọÀyè
- 1 ẹyọÀyè
- 1 ẹyọÀyè
- Àyè
- 1 ẹyọÀyè
Ìtọ́nisọ́nà yìí ń ṣe
Blueprint tó jọra
Àwọn blueprint wọ̀nyí pín ìmọ̀ — ọ̀nà, ohun-èlò tàbí ìlànà

Forge Welding Iron — Joining Two Pieces into One
láti ọwọ́ Forge
Wélídì
78
0
0
0
3
0

Upsetting: Making It Thicker by Making It Shorter
láti ọwọ́ Forge
Àwọn Irinṣẹ́ Irin
53
0
0
0
0
0

Steeled Picks: Common Pick, Pickaxe and Miner's Pick, Iron Eye with Steel Points Welded In (Edwinson, 1886)
láti ọwọ́ Forge
Iṣẹ́ Irin
11
0
0
0
0
0
CC0 Àgbègbè Gbogbogbò
Blueprint yìí ti jáde lábẹ́ CC0. O lè ṣe àdàkọ, yí padà, pín, àti lò láìsí ìyọ̀ǹda.