Ferrite Toroid Core: Magnesium-Zinc Ferrite, One-Day Grind, 1400 °C (Snoek 1948, Ex. II)
Charlie

Ṣẹ́dá nipasẹ̀

Charlie

28. Oṣù Kẹwà 2026DE
2
0
0
0
0

Ferrite Toroid Core: Magnesium-Zinc Ferrite, One-Day Grind, 1400 °C (Snoek 1948, Ex. II)

A soft ferrite ring core of magnesium-zinc ferrite: magnesia, zinc oxide and iron oxide ground for a whole day, pressed into a ring and fired at 1400 °C in oxygen. Snoek's ring had an initial permeability of 670 and a Curie point near 100 °C. Source: J. L. Snoek, US 2,452,530 (Philips, 1948), Example II. The violet iron oxide has its own blueprint (precipitated hematite calcined at 1000-1100 °C, after Nurdini et al. 2022); Snoek does not say how his was made. Picture: the patent's Fig. 4, the ring core.
Ilọsíwájú
2 days

Ìlànà

1

Weigh 25.5 : 25.5 : 49 mol %

Mix 25½ mol % pure magnesia, 25½ mol % pure zinc oxide and 49 mol % pure violet iron oxide. Ours, by weight: 9.4 g magnesium oxide, 18.99 g zinc oxide and 71.61 g iron oxide per 100 g. Snoek does not say what makes it 'violet'; violet iron oxide has its own blueprint.

Àwọn ohun èlò fún ìgbésẹ̀ yìí:

Ọ́sáídì magnesiumỌ́sáídì magnesium9.4 g
Lulú Sínkì Ọ́ksídìLulú Sínkì Ọ́ksídì18.99 g
Iron oxide aláwọ̀ àlùkòIron oxide aláwọ̀ àlùkò71.61 g

Àwọn irinṣẹ́ tí a nílò:

Òǹwọ̀n ìdọ́gbaÒǹwọ̀n ìdọ́gba
Ìbòjú ErukuÌbòjú Eruku
2

Grind for one day in an iron ball mill

Grind the mixture for one day in a mill with iron balls.

Àwọn irinṣẹ́ tí a nílò:

Ẹ̀rọ Lílọ Bọ́ọ̀lù IrinẸ̀rọ Lílọ Bọ́ọ̀lù Irin
Ìbòjú ErukuÌbòjú Eruku
3

Press a ring at 4 tons per cm²

Press the powder at 4 tons per square centimetre into a ring 3 cm across with a 4 × 4 mm cross-section.

Àwọn irinṣẹ́ tí a nílò:

Ẹ̀rọ ìtẹ̀ háídírọ́líìkìẸ̀rọ ìtẹ̀ háídírọ́líìkì
Ìdà Títẹ̀ ÒrùkaÌdà Títẹ̀ Òrùka
Ìbòjú ErukuÌbòjú Eruku
4

Fire 1 hour at 1400 °C, cool slowly in oxygen

Heat the ring in oxygen for 1 hour at 1400 °C, then cool it slowly in oxygen. Snoek's ring had an initial permeability of 670 at room temperature and 2 kHz.

Àwọn irinṣẹ́ tí a nílò:

Ààrò Ọ̀pọ́nÀàrò Ọ̀pọ́n
OxygenOxygen
Àgbá gáàsì tí a fi ìfúnpá kúnÀgbá gáàsì tí a fi ìfúnpá kún
PirómítàPirómítà
Ẹmú Ìkòkò Ìyọ́Ẹmú Ìkòkò Ìyọ́
Ìbọ̀wọ́ Tí Ń Fara Da OoruÌbọ̀wọ́ Tí Ń Fara Da Ooru

Àwọn ohun-èlò

3

Àwọn irinṣẹ́ tó nílò

11

Ìtọ́nisọ́nà yìí ń ṣe

CC0 Àgbègbè Gbogbogbò

Blueprint yìí ti jáde lábẹ́ CC0. O lè ṣe àdàkọ, yí padà, pín, àti lò láìsí ìyọ̀ǹda.

Ṣàtìlẹ́yìn Olùṣẹ́dá nípa rírà àwọn ọjà nipasẹ̀ Blueprint wọn Ẹ̀san Olùṣẹ́dá tí àwọn Olùtajà gbé kalẹ̀, tàbí ṣẹ̀dá àtúnṣe tuntun ti Blueprint yìí kí o sì fi sínú Blueprint rẹ gẹ́gẹ́ bí ìsopọ̀ láti pín owó-wíwọlé.

Ìfọ̀rọ̀wérọ̀

(0)

Wọlé láti dara pọ̀ mọ́ ìfọ̀rọ̀wérọ̀

Ń gbé àwọn ọ̀rọ̀ wọlé...