Hafnium: Iodide Vapour Split on a Tungsten Wire Heated beyond 1600 °C (van Arkel and de Boer, US 1,671,213)
Charlie

Ṣẹ́dá nipasẹ̀

Charlie

1. Oṣù Kọkànlá 2026DE
1
0
0
0
0

Hafnium: Iodide Vapour Split on a Tungsten Wire Heated beyond 1600 °C (van Arkel and de Boer, US 1,671,213)

Hafnium will not come out of its chloride and hydrogen as clean metal. Van Arkel and de Boer instead let the vapour of hafnium iodide pass a white-hot wire in an evacuated vessel: the iodide splits and pure hafnium grows on the wire. Result: hafnium metal deposited on the wire. Source: A. E. van Arkel and J. H. de Boer, US 1,671,213 (1928). The wire runs white-hot; iodine vapour is released. Picture: the patent drawing.
Ilọsíwájú
1 day

Ìlànà

1

Set up the vessel and wire

Hang a wire, for example of tungsten, inside the vessel, fixed with small screws to two leading-in wires sealed through its narrowed top. A side tube goes to a pump. For the high temperatures the iodides need, the patent advises a vessel of suitable metal such as chrome iron rather than glass.

Àwọn irinṣẹ́ tí a nílò:

Ohun èlò dígíOhun èlò dígí
Wáyà tungstenWáyà tungsten
Orísun iná DCOrísun iná DC
2

Pump out the air

Put the hafnium iodide in the vessel and pump out the air and any other gas that would spoil the reaction.

Àwọn ohun èlò fún ìgbésẹ̀ yìí:

Háfníọ̀mù iodideHáfníọ̀mù iodide1 as required

Àwọn irinṣẹ́ tí a nílò:

Ẹ̀rọ ìfàfẹ́fẹ́jádeẸ̀rọ ìfàfẹ́fẹ́jáde
3

Evaporate the iodide

Heat the vessel until the iodide gives enough vapour. The patent gives 400-600 °C only for zirconium iodide; for hafnium iodide the temperature is not given. Ours: a furnace round the vessel.

Àwọn irinṣẹ́ tí a nílò:

Ààrò Ọ̀pọ́nÀàrò Ọ̀pọ́n
4

Deposit hafnium on the white-hot wire

Pass a current through the wire to heat it beyond 1600 °C while the iodide vapour flows along it. The iodide splits and hafnium deposits on the wire. Do not overheat: the deposit can alloy with the wire.

Àwọn irinṣẹ́ tí a nílò:

Orísun iná DCOrísun iná DC
PirómítàPirómítà
Wáyà tungstenWáyà tungsten

Àwọn ohun-èlò

1

Àwọn irinṣẹ́ tó nílò

6

Ìtọ́nisọ́nà yìí ń ṣe

CC0 Àgbègbè Gbogbogbò

Blueprint yìí ti jáde lábẹ́ CC0. O lè ṣe àdàkọ, yí padà, pín, àti lò láìsí ìyọ̀ǹda.

Ṣàtìlẹ́yìn Olùṣẹ́dá nípa rírà àwọn ọjà nipasẹ̀ Blueprint wọn Ẹ̀san Olùṣẹ́dá tí àwọn Olùtajà gbé kalẹ̀, tàbí ṣẹ̀dá àtúnṣe tuntun ti Blueprint yìí kí o sì fi sínú Blueprint rẹ gẹ́gẹ́ bí ìsopọ̀ láti pín owó-wíwọlé.

Ìfọ̀rọ̀wérọ̀

(0)

Wọlé láti dara pọ̀ mọ́ ìfọ̀rọ̀wérọ̀

Ń gbé àwọn ọ̀rọ̀ wọlé...