PLA Pellets: Purified Lactide Polymerised with a Trace of Litharge
Charlie

Ṣẹ́dá nipasẹ̀

Charlie

19. Oṣù Kẹwà 2026DE
13
0
0
0
0

PLA Pellets: Purified Lactide Polymerised with a Trace of Litharge

PLA (polylactide) is the polymer of lactic acid, the stock for PLA filament. Schneider's du Pont patent (US 2,703,316, 1955) made a tough, clear polymer by heating very pure lactide with a trace of litharge in a closed, evacuated vessel: at 180 °C it was done in 6½ hours. Above 200 °C the polymer falls back to lactide. Extruding it and cutting the strand into pellets is our step. The picture: our diagram.
Ilọsíwájú
About 8 hours

Ìlànà

1

Charge lactide and litharge

Weigh 10 parts of purified lactide (melting at 125 °C in the patent's example; it must melt at 120 °C or above) and 0.004 part litharge into the reaction vessel.

Àwọn ohun èlò fún ìgbésẹ̀ yìí:

LactideLactide10 parts

Àwọn irinṣẹ́ tí a nílò:

Oxide òjé (litharge)Oxide òjé (litharge)
Òǹwọ̀n ìdọ́gbaÒǹwọ̀n ìdọ́gba
Ìkòkò ìṣesí ìfúnpáÌkòkò ìṣesí ìfúnpá
Ẹ̀rọ Ìmí P100Ẹ̀rọ Ìmí P100
2

Evacuate and close

Pump the air out of the vessel and close it.

Àwọn irinṣẹ́ tí a nílò:

Ẹ̀rọ ìfàfẹ́fẹ́jádeẸ̀rọ ìfàfẹ́fẹ́jáde
Ẹ̀rọ ìwọ̀n àìsí afẹ́fẹ́Ẹ̀rọ ìwọ̀n àìsí afẹ́fẹ́
Ìkòkò ìṣesí ìfúnpáÌkòkò ìṣesí ìfúnpá
3

Heat 6½ hours at 180 °C

Heat at 180 °C for 6½ hours. Do not go above 200 °C, where the polymer turns back to lactide. The product is a clear, colourless polymer (the example's softened at about 82 °C).

Àwọn irinṣẹ́ tí a nílò:

Ààrò ìgbẹ̀Ààrò ìgbẹ̀
Ẹ̀rọ Ìwọ̀n Ooru Yàrá ÌwádìíẸ̀rọ Ìwọ̀n Ooru Yàrá Ìwádìí
Ìkòkò ìṣesí ìfúnpáÌkòkò ìṣesí ìfúnpá
4

Extrude and pelletise

Ours: take the polymer out, melt it through an extruder and cut the cooled strand into pellets.

Àwọn irinṣẹ́ tí a nílò:

Ẹ̀rọ ìtújáde ṣíṣuẸ̀rọ ìtújáde ṣíṣu
Ẹ̀rọ Ìṣe Pẹ́lẹ́ẹ̀tìẸ̀rọ Ìṣe Pẹ́lẹ́ẹ̀tì
Ìbọ̀wọ́ Tí Ń Fara Da OoruÌbọ̀wọ́ Tí Ń Fara Da Ooru

Àwọn ohun-èlò

1
  • 10 parts
    Àyè

Àwọn irinṣẹ́ tó nílò

11

CC0 Àgbègbè Gbogbogbò

Blueprint yìí ti jáde lábẹ́ CC0. O lè ṣe àdàkọ, yí padà, pín, àti lò láìsí ìyọ̀ǹda.

Ṣàtìlẹ́yìn Olùṣẹ́dá nípa rírà àwọn ọjà nipasẹ̀ Blueprint wọn Ẹ̀san Olùṣẹ́dá tí àwọn Olùtajà gbé kalẹ̀, tàbí ṣẹ̀dá àtúnṣe tuntun ti Blueprint yìí kí o sì fi sínú Blueprint rẹ gẹ́gẹ́ bí ìsopọ̀ láti pín owó-wíwọlé.

Ìfọ̀rọ̀wérọ̀

(0)

Wọlé láti dara pọ̀ mọ́ ìfọ̀rọ̀wérọ̀

Ń gbé àwọn ọ̀rọ̀ wọlé...