PTFE Rod: a Plug Sintered in Boiling Retene Vapour (Brubaker & Hanford 1946)
Emma

Ṣẹ́dá nipasẹ̀

Emma

27. Oṣù Kẹwà 2026SE
9
0
0
0
0

PTFE Rod: a Plug Sintered in Boiling Retene Vapour (Brubaker & Hanford 1946)

The first example of du Pont's way to shape PTFE: press a small rod of powder cold, then heat it above 327 °C out of the mould. Here the heat comes from the vapour of boiling retene, which boils at 394 °C, so the temperature holds steady by itself. The plug comes out sintered into one tough piece. Source: M. M. Brubaker and W. E. Hanford (du Pont), US 2,400,099 (1946), Example I. The pressure is the patent's usual range, as the example gives none. The mould, press and the vapour-bath set-up are ours. Picture drawn by Youblob.
Ilọsíwájú
1 day

Ìlànà

1

Press a plug from the powder

At room temperature, press small particles of PTFE in a mould into a plug 0.5 in across and 0.7 in long. The example gives no pressure; the patent's usual range is 100–3000 lb/sq in.

Àwọn ohun èlò fún ìgbésẹ̀ yìí:

Erùpẹ̀ resini PTFEErùpẹ̀ resini PTFE1 as required for the plug

Àwọn irinṣẹ́ tí a nílò:

Àwòṣe ìtẹ̀mọ́lẹ̀Àwòṣe ìtẹ̀mọ́lẹ̀
Ẹ̀rọ ìtẹ̀ háídírọ́líìkìẸ̀rọ ìtẹ̀ háídírọ́líìkì
Ìdíwọ̀nÌdíwọ̀n
2

Set up a retene vapour bath

Boil retene so its vapour fills the space round a glass tube. Ours: retene in a flask on a burner, a reflux condenser on top, and the tube standing in the vapour.

Àwọn irinṣẹ́ tí a nílò:

ReteneRetene
Ìgò Gíláàsì ÌsànÌgò Gíláàsì Ìsàn
Kọ́ndẹ́nsà Ìpadàbọ̀Kọ́ndẹ́nsà Ìpadàbọ̀
Ọ̀gọ̀ BunsenỌ̀gọ̀ Bunsen
Àwọn tube ìdánwòÀwọn tube ìdánwò
3

Sinter for 3 hours

Take the plug out of the mould, put it in the glass tube, and heat it in the vapour of boiling retene (394 °C) for 3 hours.

Àwọn irinṣẹ́ tí a nílò:

Àwọn tube ìdánwòÀwọn tube ìdánwò
ReteneRetene
Ọ̀gọ̀ BunsenỌ̀gọ̀ Bunsen
4

Cool it under the retene

Remove the heat source and let the plug cool where it is. It is now sintered together into a tough mass.

Àwọn irinṣẹ́ tí a nílò:

Àwọn tube ìdánwòÀwọn tube ìdánwò

Àwọn ohun-èlò

1

Àwọn irinṣẹ́ tó nílò

8

Ìtọ́nisọ́nà yìí ń ṣe

CC0 Àgbègbè Gbogbogbò

Blueprint yìí ti jáde lábẹ́ CC0. O lè ṣe àdàkọ, yí padà, pín, àti lò láìsí ìyọ̀ǹda.

Ṣàtìlẹ́yìn Olùṣẹ́dá nípa rírà àwọn ọjà nipasẹ̀ Blueprint wọn Ẹ̀san Olùṣẹ́dá tí àwọn Olùtajà gbé kalẹ̀, tàbí ṣẹ̀dá àtúnṣe tuntun ti Blueprint yìí kí o sì fi sínú Blueprint rẹ gẹ́gẹ́ bí ìsopọ̀ láti pín owó-wíwọlé.

Ìfọ̀rọ̀wérọ̀

(0)

Wọlé láti dara pọ̀ mọ́ ìfọ̀rọ̀wérọ̀

Ń gbé àwọn ọ̀rọ̀ wọlé...