Teaspoon Sawn Short from Silver Sheet, Then Hammered Out (Payne 1914)
Saw the spoon out of flat silver smaller than it will end up: shorter, narrower in the bowl and thicker in the shank. Hammering then stretches it to full size. Arthur Payne said this method was used largely for silver teaspoons.
Source: A. F. Payne, Art Metalwork with Inexpensive Equipment (1914), pp. 180–184; annealing from his chapter XI. The millimetre figure is ours. Picture: Payne's Fig. 155, the blank and the finished spoon.
Àárín
1 day
Ìlànà
1
1
Saw out the short blank
Saw out the short blank
Mark out and saw the blank from 15-gauge sterling silver (about 1.45 mm; our conversion): 5 in long, the bowl 1⅛ in wide and the shank 5⁄16 in wide. The finished spoon will be 6 in long with a bowl 1⅝ in wide.
Àwọn ohun èlò fún ìgbésẹ̀ yìí:
Abala Fàdákà Sítẹ́líìnì1 piece 15 gauge, enough for the 5 in blankÀwọn irinṣẹ́ tí a nílò:
Abẹ́rẹ́ Ìkọ Ìlà
Ayùn Alágbẹ̀dẹ Wúrà2
2
Stretch the bowl wider
Stretch the bowl wider
Hammer the bowl on a flat anvil with the ball-pein hammer, held at a slight angle towards the side you want it to grow. This makes the bowl thinner and wider.
Àwọn irinṣẹ́ tí a nílò:
Ìdí Alágbẹ̀dẹ
Òòlù olórí bọ́ọ̀lù3
3
Narrow the shank with the neck hammer
Narrow the shank with the neck hammer
Hold the spoon on edge on a rounded convex stake and hammer the shank narrower with the neck hammer. This lengthens the spoon and makes the shank narrower and thicker. Widen the tip of the handle the same way as the bowl.
Àwọn irinṣẹ́ tí a nílò:
Igi tí a gún
Òòlù ọrùn
Òòlù olórí bọ́ọ̀lù4
4
Anneal and repeat
Anneal and repeat
When the silver gets hard, heat it to a dull red and plunge it into water, or let it cool. Repeat the hammering and annealing until the spoon is roughly to shape.
Àwọn ohun èlò fún ìgbésẹ̀ yìí:
Omi1 as requiredÀwọn irinṣẹ́ tí a nílò:
Ọ̀gọ̀ Bunsen
Ẹ̀mú
Ohun èlò dígí5
5
File and planish
File and planish
File the rough edges smooth, then planish the whole spoon carefully.
Àwọn irinṣẹ́ tí a nílò:
Àwọn Ìfá (Ìfá Ọwọ́)
Òòlù ìdán
Igi tí a gún6
6
Polish out the file marks
Polish out the file marks
Rub out all the scratches and file marks with emery cloth.
Àwọn irinṣẹ́ tí a nílò:
Aṣọ emery7
7
Anneal to even the fire scale
Anneal to even the fire scale
Anneal the spoon thoroughly once more. Heated silver grows a thin white skin, the fire scale, and this brings it back over the spots where filing and polishing took it off, so the colour is even.
Àwọn ohun èlò fún ìgbésẹ̀ yìí:
Omi1 as requiredÀwọn irinṣẹ́ tí a nílò:
Ọ̀gọ̀ Bunsen
Ẹ̀mú
Ohun èlò dígí8
8
Planish with smooth hammers
Planish with smooth hammers
Planish the spoon on smooth tools with smooth, bright hammers. This makes it stiff again after the annealing.
Àwọn irinṣẹ́ tí a nílò:
Òòlù ìdán
Ìdí Alágbẹ̀dẹ
Igi tí a gún9
9
Final polish with rouge
Final polish with rouge
Polish it lightly with a soft cotton flannel and a little red rouge.
Àwọn irinṣẹ́ tí a nílò:
Aṣọ ìfọ́ ohun ọ̀ṣọ́
Pupa ìdán alágbẹ̀dẹ wúràÀwọn ohun-èlò
2- 1 piece 15 gauge, enough for the 5 in blankÀyè
- 2 as requiredÀyè
Àwọn irinṣẹ́ tó nílò
14- Àyè
- Àyè
- Àyè
- Àyè
- Àyè
- Àyè
Ìtọ́nisọ́nà yìí ń ṣe
Blueprint tó jọra
Àwọn blueprint wọ̀nyí pín ìmọ̀ — ọ̀nà, ohun-èlò tàbí ìlànà
CC0 Àgbègbè Gbogbogbò
Blueprint yìí ti jáde lábẹ́ CC0. O lè ṣe àdàkọ, yí padà, pín, àti lò láìsí ìyọ̀ǹda.
Ṣàtìlẹ́yìn Olùṣẹ́dá nípa rírà àwọn ọjà nipasẹ̀ Blueprint wọn Ẹ̀san Olùṣẹ́dá tí àwọn Olùtajà gbé kalẹ̀, tàbí ṣẹ̀dá àtúnṣe tuntun ti Blueprint yìí kí o sì fi sínú Blueprint rẹ gẹ́gẹ́ bí ìsopọ̀ láti pín owó-wíwọlé.