Tinned Copper Wire: Boiled with Cream of Tartar and Grain Tin (Spon's Workshop Receipts)
Copper wire tinned without melting any tin: grain tin or tin shavings are boiled with cream of tartar and water, and the copper boiled in the same liquor until tin comes down on it as metal.
Spon gives the receipt for copper and brass in general. Here the copper is wire. Not given: how long to boil.
Source: Spon, Workshop Receipts, first series, p. 336. Picture: the receipt.
Olùbẹ̀rẹ̀
Unknown
Ìlànà
1
1
Boil the tinning liquor
Boil the tinning liquor
Boil 6 lb of cream of tartar, 4 gallons of water and 8 lb of grain tin or tin shavings together for a sufficient time. Ours: a clay pot as the vessel.
Àwọn ohun èlò fún ìgbésẹ̀ yìí:
Ìpara tartar1 6 lb
Omi1 4 gallons
Ìdì tin1 8 lb, as grain or shavingsÀwọn irinṣẹ́ tí a nílò:
Ìkòkò amọ̀2
2
Boil the wire in it
Boil the wire in it
Put the copper wire into the liquor and keep it boiling. The tin is precipitated on the copper in its metallic form.
Àwọn ohun èlò fún ìgbésẹ̀ yìí:
Okùn Bàbà1 ẹyọÀwọn irinṣẹ́ tí a nílò:
Ìkòkò amọ̀Àwọn ohun-èlò
4- 1 6 lbÀyè
- 1 4 gallonsÀyè
- 1 8 lb, as grain or shavingsÀyè
- 1 ẹyọÀyè
Àwọn irinṣẹ́ tó nílò
1- Àyè
Ìtọ́nisọ́nà yìí ń ṣe
CC0 Àgbègbè Gbogbogbò
Blueprint yìí ti jáde lábẹ́ CC0. O lè ṣe àdàkọ, yí padà, pín, àti lò láìsí ìyọ̀ǹda.
Ṣàtìlẹ́yìn Olùṣẹ́dá nípa rírà àwọn ọjà nipasẹ̀ Blueprint wọn Ẹ̀san Olùṣẹ́dá tí àwọn Olùtajà gbé kalẹ̀, tàbí ṣẹ̀dá àtúnṣe tuntun ti Blueprint yìí kí o sì fi sínú Blueprint rẹ gẹ́gẹ́ bí ìsopọ̀ láti pín owó-wíwọlé.