Two-Part Epoxy Glue: Bis-Phenol Resin Thinned with Allyl Glycidyl Ether, Hardened with Diethylene Triamine
Woody

Ṣẹ́dá nipasẹ̀

Woody

18. Oṣù Kẹwà 2026NO
13
0
0
0
0

Two-Part Epoxy Glue: Bis-Phenol Resin Thinned with Allyl Glycidyl Ether, Hardened with Diethylene Triamine

Bis-phenol epoxy resin is too thick to spread, so it is thinned with a fifth of its weight of allyl glycidyl ether, which joins the cure. That is part A; part B is diethylene triamine. Stir 10 parts of B into 100 of A, spread, join, and it hardens at room temperature: after six days at 25 °C, block joints held 3,550 lb/in² (Wiles and Newey, Shell, US 2,528,932, 1950). It bonds wood, metal and resins. The picture: our drawing of the two bottles and a glued joint.
Àárín
A week to full strength

Ìlànà

1

Make part A

Warm 400 g bis-phenol epoxy resin until it flows (our step; it softens at 43 °C) and stir in 100 g allyl glycidyl ether, to a smooth, spreadable syrup. Bottle it.

Àwọn ohun èlò fún ìgbésẹ̀ yìí:

Resini epoxy bisphenolResini epoxy bisphenol400 g
Allyl glycidyl etherAllyl glycidyl ether100 g

Àwọn irinṣẹ́ tí a nílò:

Ago BórósílíkéètìAgo Bórósílíkéètì
Pátákó GbígbónáPátákó Gbígbóná
Ohun ìrúwéOhun ìrúwé
Ẹ̀rọ Ìwọ̀n OoruẸ̀rọ Ìwọ̀n Ooru
Òṣùwọ̀n Díjítà Ilé ÌdánáÒṣùwọ̀n Díjítà Ilé Ìdáná
Ìgò dígí tí ó ní ìdéríÌgò dígí tí ó ní ìdérí
Ìbọ̀wọ́ rọ́bàÌbọ̀wọ́ rọ́bà
2

Bottle part B

Bottle diethylene triamine separately and keep it closed: it is strongly alkaline and burns skin. You need 10 g for every 100 g of part A.

Àwọn ohun èlò fún ìgbésẹ̀ yìí:

Diethylene triamineDiethylene triamine50 g

Àwọn irinṣẹ́ tí a nílò:

Ìgò dígí tí ó ní ìdéríÌgò dígí tí ó ní ìdérí
Ìbọ̀wọ́ rọ́bàÌbọ̀wọ́ rọ́bà
3

Mix only what you need

Weigh part A into a cup, add a tenth of its weight of part B, and stir well. It begins to cure at once, so mix just before gluing.

Àwọn irinṣẹ́ tí a nílò:

Kọ́ọ̀bù ìdíwọ̀nKọ́ọ̀bù ìdíwọ̀n
Òṣùwọ̀n Díjítà Ilé ÌdánáÒṣùwọ̀n Díjítà Ilé Ìdáná
Ohun ìrúwéOhun ìrúwé
Ìbọ̀wọ́ rọ́bàÌbọ̀wọ́ rọ́bà
4

Spread, join, wait

Spread a thin coat on both faces and press them together. At room temperature it sets in half an hour to a day and reaches full strength in one to two weeks; warmth speeds it up.

Àwọn irinṣẹ́ tí a nílò:

Búrọ́ọ̀ṣì gọ́mùBúrọ́ọ̀ṣì gọ́mù
5

Mixing table

Ń ṣí ìwé Jupyter…

Àwọn ohun-èlò

3

Àwọn irinṣẹ́ tó nílò

9

Ìtọ́nisọ́nà yìí ń ṣe

CC0 Àgbègbè Gbogbogbò

Blueprint yìí ti jáde lábẹ́ CC0. O lè ṣe àdàkọ, yí padà, pín, àti lò láìsí ìyọ̀ǹda.