Violet Iron Oxide: Precipitated Hematite Calcined at 1000-1100 °C (Nurdini et al. 2022)
Charlie

Ṣẹ́dá nipasẹ̀

Charlie

1. Oṣù Kọkànlá 2026DE
1
0
0
0
0

Violet Iron Oxide: Precipitated Hematite Calcined at 1000-1100 °C (Nurdini et al. 2022)

Iron hydroxide is thrown down from hot ferric nitrate solution with ammonia, washed, dried and calcined. All of it ends as pure hematite, but the colour moves from bright red through dark red to purple as the calcining heat rises from 1000 °C, because the grains grow larger and more crystalline. Result: pure violet to purple ferric oxide (hematite) after 4 hours at 1000-1100 °C. Source: Nurdini et al., Heliyon 8 (2022) e10377, sections 2.2 and 4. Not given: batch size, how much ammonia, end pH, yield. Picture drawn by Youblob.
Àárín
2 days

Ìlànà

1

Heat the ferric nitrate solution

Make a 0.05 M solution of ferric nitrate in distilled water and heat it to 80 °C.

Àwọn ohun èlò fún ìgbésẹ̀ yìí:

Ferric nitrateFerric nitrate1 as required

Àwọn irinṣẹ́ tí a nílò:

Omi Àyọ́Omi Àyọ́
Ago GílásìAgo Gílásì
Pátákó GbígbónáPátákó Gbígbóná
Ẹ̀rọ Ìwọ̀n OoruẸ̀rọ Ìwọ̀n Ooru
2

Throw down the hydroxide with ammonia

Keeping it at 80 °C, add ammonia solution drop by drop while stirring well. Stir for 3 hours, then let it cool to room temperature: a red-brown precipitate forms. Not given: how much ammonia.

Àwọn irinṣẹ́ tí a nílò:

Omi amonia - 25-28 %Omi amonia - 25-28 %
Fọ́nẹ́ẹ̀lì Ìsọ̀kalẹ̀ ÌkánFọ́nẹ́ẹ̀lì Ìsọ̀kalẹ̀ Ìkán
Pátákó GbígbónáPátákó Gbígbóná
Ẹ̀rọ Ìwọ̀n OoruẸ̀rọ Ìwọ̀n Ooru
3

Spin down, wash and dry

Collect the precipitate in a centrifuge at 4000 rpm for 15 minutes, wash it with distilled water, and dry it at 110 °C for 24 hours.

Àwọn irinṣẹ́ tí a nílò:

Centrifuge orí tábìlìCentrifuge orí tábìlì
Omi Àyọ́Omi Àyọ́
Ààrò ìgbẹ̀Ààrò ìgbẹ̀
4

Calcine at 1000-1100 °C

Calcine for 4 hours in air at 1000-1100 °C. Below 1000 °C it stays bright or dark red; from 1000 °C it turns purple. Grind the cooled oxide to a fine powder (they used an agate mortar).

Àwọn irinṣẹ́ tí a nílò:

Ààrò muffleÀàrò muffle
Odó àti Ọmọ OdóOdó àti Ọmọ Odó

Àwọn ohun-èlò

1

Àwọn irinṣẹ́ tó nílò

10

Ìtọ́nisọ́nà yìí ń ṣe

CC0 Àgbègbè Gbogbogbò

Blueprint yìí ti jáde lábẹ́ CC0. O lè ṣe àdàkọ, yí padà, pín, àti lò láìsí ìyọ̀ǹda.

Ṣàtìlẹ́yìn Olùṣẹ́dá nípa rírà àwọn ọjà nipasẹ̀ Blueprint wọn Ẹ̀san Olùṣẹ́dá tí àwọn Olùtajà gbé kalẹ̀, tàbí ṣẹ̀dá àtúnṣe tuntun ti Blueprint yìí kí o sì fi sínú Blueprint rẹ gẹ́gẹ́ bí ìsopọ̀ láti pín owó-wíwọlé.

Ìfọ̀rọ̀wérọ̀

(0)

Wọlé láti dara pọ̀ mọ́ ìfọ̀rọ̀wérọ̀

Ń gbé àwọn ọ̀rọ̀ wọlé...