Wool Flock: Raw Wool Scoured in Soda Suds and Hand-Carded for Stuffing (USDA, 1933)
Tex

Nilikha ni

Tex

22. Nobyembre 2026FO
22
0
0
0
0

Wool Flock: Raw Wool Scoured in Soda Suds and Hand-Carded for Stuffing (USDA, 1933)

Loose wool stuffing for saddle panels, collars and pads from your own raw fleece: picked over, scoured in warm soap and sal-soda suds without stirring, rinsed, dried in the sun and carded open. The method is the U.S. Bureau of Home Economics leaflet of 1933 for preparing raw wool at home.
Baguhan
One day, plus drying

Mga Tagubilin

1

Scouring a raw fleece

A raw fleece washed by hand (Marina Skua). The USDA method below uses three soap suds and three rinses.
2

The 1933 leaflet

USDA Bureau of Home Economics, "How to Prepare Raw Wool at Home for Bedding" (1933): scour small lots in soft water, never stir or squeeze, rinse three times, dry thoroughly and card. Expect the wool to lose 45 to 65 per cent of its weight.
Hakbang 2 - Image 1
3

Read the leaflet

The 1933 leaflet (two pages, public domain).
File ng DisenyoPDFCC0 - Free
4

Pick the fleece over

Take only the cleanest of the fleece. Pick it apart, shaking out all the dirt you can, and remove all tags and dung locks; stained wool will not scour white.

Mga materyales para sa hakbang na ito:

Hilaw na balahibo ng tupaHilaw na balahibo ng tupa1 kg
5

Make the stock soap

Heat slowly 1 lb (450 g) sal-soda and 2 lb (900 g) of a good neutral soap, not strong laundry soap, in 2 gallons (7.6 l) of soft water, then fill up to 5 gallons (19 l).

Mga materyales para sa hakbang na ito:

Sodang panlabaSodang panlaba450 g
SabonSabon900 g
TubigTubig19 l

Mga kailangang kasangkapan:

BaldeBalde
6

Scour in three suds

First suds: 1 to 2 quarts (1-2 l) of stock soap in 10 gallons (38 l) of water at about 120 F (49 C), uncomfortable but bearable. Second and third: a little cooler, 110-120 F (43-49 C), with less soap; if the wool is very clean, soda in the first only. Use about 6 gallons of suds per pound of wool (50 l per kg) and never crowd it. Push the wool under with the paddle, let it stand about 10 minutes without stirring or squeezing, lift small amounts, drain and pass them through the wringer.

Mga materyales para sa hakbang na ito:

TubigTubig150 l

Mga kailangang kasangkapan:

BaldeBalde
Sagwan na kahoySagwan na kahoy
Pampiga ng damit na may rolyoPampiga ng damit na may rolyo
Termometrong pangkusinaTermometrong pangkusina
7

Rinse and dry

Rinse at least three times in soft water at the temperature of the last suds, handled the same way; add 1 to 2 pints (0.5-1 l) of vinegar to the last rinse. Spread it thinly on boards covered with clean sheets in the sun, raised on horses with gaps for air, and dry it thoroughly.

Mga materyales para sa hakbang na ito:

TubigTubig120 l
SukaSuka1 l

Mga kailangang kasangkapan:

BaldeBalde
Sagwan na kahoySagwan na kahoy
Pampiga ng damit na may rolyoPampiga ng damit na may rolyo
Pantuyuang EstantePantuyuang Estante
8

Card it open

Card the dry wool with hand cards to straighten the fibres and take out the small bits of chaff. Store it loose, protected from moths, and use it as stuffing.

Mga kailangang kasangkapan:

Suklay ng lanaSuklay ng lana
9

Troubleshooting

Wool problems and fixes.

Flow

Loading...
10

History and honest limits

From the U.S. Department of Agriculture, Bureau of Home Economics leaflet 478R, "How to Prepare Raw Wool at Home for Bedding" (21 October 1933), written for comforters and mattresses; the same clean carded wool is the flock harness makers stuff panels with. Ours: the metric figures. Photo: Wikipedista:Ryj, public domain. Not made by us yet.

Mga Materyales

5
  • Placeholder
  • Placeholder
  • 900 g
    Placeholder
  • 289 l
    Placeholder
  • 1 l
    Placeholder

Mga Kinakailangang Kasangkapan

6

Mga design file

1

Ang blueprint na ito ay gumagawa ng

Kaugnay na Blueprint

Ang mga blueprint na ito ay nagbabahagi ng kaalaman — mga teknik, materyales, o prinsipyo

CC0 Pampublikong Domain

Ang blueprint na ito ay inilabas sa ilalim ng CC0. Malaya kang kumopya, magbago, mamahagi, at gumamit nang walang pahintulot.