Black Cobbler's Wax: Resin and Pitch With Linseed Oil, Pulled to Golden Colour (Hasluck, Harness Making, 1904)
Forge

Nilikha ni

Forge

14. Nobyembre 2026NO
19
0
0
0
0

Black Cobbler's Wax: Resin and Pitch With Linseed Oil, Pulled to Golden Colour (Hasluck, Harness Making, 1904)

The saddler's black wax for waxed threads, from P. N. Hasluck's Harness Making (1904): half a pound each of resin and pitch melted together, softened with boiled linseed oil to suit the season, poured into cold water and pulled by wet hands until golden and until a piece floats. It makes about thirty lumps, kept under water.
Baguhan
About 1 hour

Mga Tagubilin

1

Batch in grams

Naglo-load ng Jupyter notebook…
2

Read Harness Making

"Black cobbler's wax is made by melting together 1/2 lb. each of resin and pitch."
3

Melt and oil

Melt 1/2 lb of resin and 1/2 lb of pitch together and mix thoroughly. Take the pan off the fire and add boiled linseed oil, about a pennyworth or less: only half as much in summer as in winter, more the colder it is. Mix well.

Mga materyales para sa hakbang na ito:

Dagta ng PinoDagta ng Pino1 piraso
Brea ng alkitran ng kahoyBrea ng alkitran ng kahoy1 piraso
Pinakuluang Langis ng LinsidPinakuluang Langis ng Linsid1 piraso

Mga kailangang kasangkapan:

Malaking KalderoMalaking Kaldero
Sulô ng PropanoSulô ng Propano
Timbangang panimbangTimbangang panimbang
4

Test

Pour a little into cold water, leave it a minute, and take it out with well-wetted hands. If it cracks when worked it is too hard; if it pulls out and sticks together it is right. Do not put the tested piece back in the pan: the water in it froths the hot wax.

Mga kailangang kasangkapan:

Balde na 20 LitroBalde na 20 Litro
5

Pour and pull

Put the test piece back in the water and pour the rest in after it. Gather the wax with wet hands without delay and pull it fast, hand over hand, until it is a light golden colour. Cut off a piece with wet scissors and drop it in the water: if it floats it has been pulled enough; if it sinks, pull more. Under-pulled wax is brittle.

Mga kailangang kasangkapan:

Balde na 20 LitroBalde na 20 Litro
GuntingGunting
6

Adjust and store

If it is too hard, melt again and add oil; if too soft, add pitch and resin. Cut it into lumps the size of a large pigeon's egg (about thirty) and keep them in water.

Mga kailangang kasangkapan:

GuntingGunting
Balde na 20 LitroBalde na 20 Litro
7

Troubleshooting

Wax troubleshooting.

Flow

Loading...
8

History and honest limits

From Paul N. Hasluck, **Harness Making** (1904), "Harness-makers' Materials" (checked on the archive.org scan harnessmaking00hasl, pp. 30-31). He says only "pitch"; wood-tar pitch is our choice. His white wax, made with white lead, is left out because white lead is a poison. The metric figures and the diagram are ours.

Mga Materyales

3

Mga Kinakailangang Kasangkapan

5

Ang blueprint na ito ay gumagawa ng

Kaugnay na Blueprint

Ang mga blueprint na ito ay nagbabahagi ng kaalaman — mga teknik, materyales, o prinsipyo

CC0 Pampublikong Domain

Ang blueprint na ito ay inilabas sa ilalim ng CC0. Malaya kang kumopya, magbago, mamahagi, at gumamit nang walang pahintulot.