Aluminium Oxide Abrasive Grit: Alundum by Jacobs's Process (Stansfield, 1914)

Alundum, the artificial corundum made at Niagara Falls by the Norton Company: bauxite, calcined to drive off its water, is fused in an electric arc furnace with about 5 per cent carbon, which reduces its iron, silicon and titanium to metal nodules; the fused alumina cools slowly into a hard crystalline mass that is crushed and sized as abrasive grit. Bauxite melts near 2,000 °C and could not be melted commercially without the electric furnace. Source: A. Stansfield, The Electric Furnace, 2nd ed. (1914), pp. 357-358. Picture: the book's Fig. 143, the Higgins alundum furnace.
Abantado
Unknown

Mga Tagubilin

1

Calcine the bauxite

Calcine the bauxite in a rotary kiln to drive off its combined water.

Mga materyales para sa hakbang na ito:

BauxiteBauxite1 piraso

Mga kailangang kasangkapan:

Umiikot na pugonUmiikot na pugon
2

Fuse in the arc furnace

Strike arcs between the electrodes and the carbon lining of the furnace bottom, then feed the calcined bauxite, with about 5 per cent carbon, in round the arcs; it melts and in time carries the current between the two arcs. Lower the water-cooled shell as the fused alundum builds up; the lower part solidifies as it fills.

Mga materyales para sa hakbang na ito:

KarbonKarbon1 about 5 per cent

Mga kailangang kasangkapan:

Pugon na de-kuryenteng arkoPugon na de-kuryenteng arko
3

Cool slowly

When the shell is full, lift it with its contents off the base, put another shell in place, and let the alundum cool slowly so it grows into a hard, tough crystalline mass.

Mga kailangang kasangkapan:

Pugon na de-kuryenteng arkoPugon na de-kuryenteng arko
4

Crush, separate and size

Break up and crush the mass, separate the nodules of reduced metal mechanically, and size the grains for use as an abrasive.

Mga kailangang kasangkapan:

Pandurog ng batoPandurog ng bato
Set ng salaan (sunod-sunod na butas)Set ng salaan (sunod-sunod na butas)

Mga Materyales

2
  • 1 piraso
    Placeholder
  • 1 about 5 per cent
    Placeholder

Mga Kinakailangang Kasangkapan

4

CC0 Pampublikong Domain

Ang blueprint na ito ay inilabas sa ilalim ng CC0. Malaya kang kumopya, magbago, mamahagi, at gumamit nang walang pahintulot.

Suportahan ang Maker sa pamamagitan ng pagbili ng mga produkto sa kanilang Blueprint Komisyon ng Maker itinakda ng mga Vendor, o lumikha ng bagong bersyon ng Blueprint na ito at isama bilang koneksyon sa iyong Blueprint upang ibahagi ang kita.

Talakayan

(0)

Mag-login upang sumali sa talakayan

Naglo-load ng mga komento...