Aqueous PTFE Dispersion: Tetrafluoroethylene Polymerised in Soapy Water (Berry 1951)
Ordinary soaps stop tetrafluoroethylene from growing into long chains. A fluorine soap does not: with 2 % of ammonium dodecafluoroheptanoate in the water, the gas polymerises into tiny PTFE ribbons that stay suspended. The result is a milky dispersion, a third of it polymer, the raw material for PTFE fine powder.
Source: K. L. Berry (du Pont), US 2,559,752 (1951), Example III. Making the ammonium salt from our acid, and the apparatus, are ours. Picture drawn by Youblob.
Abantado
1 day
Mga Tagubilin
1
1
Make the ammonium salt
Make the ammonium salt
Ours: neutralise about 1.9 parts of dodecafluoroheptanoic acid with ammonia solution until just neutral to litmus, giving 2 parts of ammonium dodecafluoroheptanoate. Make it up with distilled water to 93 parts of water in all. Parts are by weight.
Mga materyales para sa hakbang na ito:
Asidong dodecafluoroheptanoic1.9 parts
Solusyon ng ammonia - 25-28 %1 as required to neutralise
Distiladong Tubig93 partsMga kailangang kasangkapan:
Papel na litmus
Sisidlang salamin
Timbangang panimbang2
2
Load the pressure vessel
Load the pressure vessel
Put the solution in a pressure vessel with 0.05 part of potassium persulfate and 5 parts of paraffin wax melting at 56–58 °C. The wax protects the colloid while it is stirred.
Mga kailangang kasangkapan:
Persulfate na pansimula ng reaksiyon
Kandilang paraffin
Reactor na may presyon
Timbangang panimbang3
3
Heat and remove the air
Heat and remove the air
Bring it to 80–85 °C, then evacuate the vessel and hold it under reduced pressure for several minutes to drive out air and dissolved oxygen.
Mga kailangang kasangkapan:
Reactor na may presyon
Bombang panghigop ng hangin
Termometro4
4
Feed tetrafluoroethylene for 3.6 hours
Feed tetrafluoroethylene for 3.6 hours
Let in tetrafluoroethylene to 60 lb/sq in gauge. Agitate at 80–85 °C for 3.6 hours; each time the pressure falls to 55 lb/sq in, bring it back to 60.
Mga materyales para sa hakbang na ito:
Tetrafluoroetilena1 as required to hold 55–60 psiMga kailangang kasangkapan:
Reactor na may presyon
Tangke ng gas na may presyon
Panukat ng Diin
Termometro5
5
Cool and lift off the wax
Cool and lift off the wax
Cool it. The paraffin sets on top and lifts off. Below it is a colloidal PTFE dispersion with 34 % solids.
Mga kailangang kasangkapan:
Reactor na may presyon
Garapong Salamin na May TakipMga Materyales
4- 1.9 partsPlaceholder
- 1 as required to neutralisePlaceholder
- 93 partsPlaceholder
- 1 as required to hold 55–60 psiPlaceholder
Mga Kinakailangang Kasangkapan
11- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- 1 vendor sell this, none ship to you yetPlaceholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
Ang blueprint na ito ay gumagawa ng
Kaugnay na Blueprint
Ang mga blueprint na ito ay nagbabahagi ng kaalaman — mga teknik, materyales, o prinsipyo

Mapanganib
Dodecafluoroheptanoic Acid: the Fluoro Alcohol Oxidised with Permanganate (Berry 1951)
ni Charlie
Industriyal
7
0
0
0
0
0

Mapanganib
Tetrafluoroethylene: Chlorodifluoromethane Pyrolysed in a Silver Tube at 700 °C
ni Charlie
Industriyal
10
0
0
0
0
0

PTFE Resin Powder: Tetrafluoroethylene Polymerised under Pressure, Plunkett 1941
ni Charlie
Industriyal
11
0
0
0
0
0
CC0 Pampublikong Domain
Ang blueprint na ito ay inilabas sa ilalim ng CC0. Malaya kang kumopya, magbago, mamahagi, at gumamit nang walang pahintulot.
Suportahan ang Maker sa pamamagitan ng pagbili ng mga produkto sa kanilang Blueprint Komisyon ng Maker itinakda ng mga Vendor, o lumikha ng bagong bersyon ng Blueprint na ito at isama bilang koneksyon sa iyong Blueprint upang ibahagi ang kita.