MGA WEARABLE
Barium-Calcium Ferrite Disc Magnet: 5 % Calcium, Sintered at 1330 °C (Went, Philips 1956, Ex. 18)
Charlie

Nilikha ni

Charlie

28. Oktubre 2026DE
2
0
0
0
0

Barium-Calcium Ferrite Disc Magnet: 5 % Calcium, Sintered at 1330 °C (Went, Philips 1956, Ex. 18)

A ceramic magnet with a twentieth of the barium replaced by calcium: 0.095 mol barium carbonate, 0.005 mol calcium carbonate and 0.6 mol iron oxide. It is milled, fired in air, milled again, pressed and passed through a 1330 °C furnace in 10 minutes. The X-ray picture showed only the magnetoplumbite phase. Went's rod held 1,680 gauss with a coercive force of 1,110 oersted. Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 18. They sintered rods; discs and the magnetising are ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Abantado
2 days

Mga Tagubilin

1

Weigh barium carbonate, chalk and iron oxide

Weigh 18.74 g barium carbonate (0.095 mol), 0.5 g calcium carbonate (0.005 mol) and 95.55 g ferric oxide (0.6 mol). The patent used analytical-grade carbonates. Barium carbonate is poisonous if swallowed: gloves and a dust respirator.

Mga materyales para sa hakbang na ito:

Barium carbonate (witherite)Barium carbonate (witherite)18.74 g
Calcium carbonate (puting tisa)Calcium carbonate (puting tisa)0.5 g
Ferric oxideFerric oxide95.55 g

Mga kailangang kasangkapan:

Timbangang panimbangTimbangang panimbang
Gwantes na gomaGwantes na goma
Panala sa Hininga na P100Panala sa Hininga na P100
2

Mill 4 hours, dry at 150 °C

Grind with alcohol in a ball mill for 4 hours and dry in air at 150 °C.

Mga kailangang kasangkapan:

Gilingang Bolang BakalGilingang Bolang Bakal
Etanol - antas laboratoryo, 95 %Etanol - antas laboratoryo, 95 %
Hurnong pantuyoHurnong pantuyo
3

Presinter in air at 1000 °C for 2 hours

Fire the dry powder in air at 1000 °C for 2 hours.

Mga kailangang kasangkapan:

Muffle furnaceMuffle furnace
Krisol na may takip (porselana)Krisol na may takip (porselana)
Sipit ng KrisolSipit ng Krisol
Guwantes na Matibay sa InitGuwantes na Matibay sa Init
4

Mill again, dry, press at 1.5 t/cm²

Grind again with alcohol for 4 hours, dry, and press at 1.5 tonnes per cm² (ours: discs instead of rods).

Mga kailangang kasangkapan:

Gilingang Bolang BakalGilingang Bolang Bakal
Etanol - antas laboratoryo, 95 %Etanol - antas laboratoryo, 95 %
Hurnong pantuyoHurnong pantuyo
Haydroliko na pandiinHaydroliko na pandiin
Hulmahan sa pagpindot ng diskHulmahan sa pagpindot ng disk
5

Pass through a 1330 °C zone in 10 minutes

Sinter at 1330 °C by passing the pieces through a 10 cm hot zone at 10 mm per minute: 10 minutes in the heat.

Mga kailangang kasangkapan:

Hurnong TuboHurnong Tubo
Guwantes na Matibay sa InitGuwantes na Matibay sa Init
6

Magnetise the discs

The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.

Mga kailangang kasangkapan:

ElektromagnetoElektromagneto
KompasKompas

Mga Materyales

3

Mga Kinakailangang Kasangkapan

15

Ang blueprint na ito ay gumagawa ng

Kaugnay na Blueprint

Ang mga blueprint na ito ay nagbabahagi ng kaalaman — mga teknik, materyales, o prinsipyo

CC0 Pampublikong Domain

Ang blueprint na ito ay inilabas sa ilalim ng CC0. Malaya kang kumopya, magbago, mamahagi, at gumamit nang walang pahintulot.

Suportahan ang Maker sa pamamagitan ng pagbili ng mga produkto sa kanilang Blueprint Komisyon ng Maker itinakda ng mga Vendor, o lumikha ng bagong bersyon ng Blueprint na ito at isama bilang koneksyon sa iyong Blueprint upang ibahagi ang kita.

Talakayan

(0)

Mag-login upang sumali sa talakayan

Naglo-load ng mga komento...