Barium-Calcium Ferrite Disc Magnet: 0.09 mol BaCO3 and 0.01 mol CaCO3 (Went, Philips 1956, Ex. 19)

A ceramic magnet with a tenth of the barium replaced by calcium: 0.09 mol barium carbonate and 0.01 mol calcium carbonate to 0.6 mol iron oxide, made as in Example 18: milled, presintered at 1000 °C, milled again, formed and passed through a 1330 °C furnace in 10 minutes. Went's rod held 1,705 gauss with a coercive force of 1,110 oersted. Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 19. They sintered rods; discs and the magnetising are ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Abantado
2 days

Mga Tagubilin

1

Weigh barium carbonate, chalk and iron oxide

Weigh 17.76 g barium carbonate (0.09 mol), 1.001 g calcium carbonate (0.01 mol) and 95.55 g ferric oxide (0.6 mol). Barium carbonate is poisonous if swallowed: gloves and a dust respirator.

Mga materyales para sa hakbang na ito:

Barium carbonate (witherite)Barium carbonate (witherite)17.76 g
Calcium carbonate (puting tisa)Calcium carbonate (puting tisa)1.001 g
Ferric oxideFerric oxide95.55 g

Mga kailangang kasangkapan:

Timbangang panimbangTimbangang panimbang
Gwantes na gomaGwantes na goma
Panala sa Hininga na P100Panala sa Hininga na P100
2

Mill with alcohol 4 hours, dry at 150 °C

Grind with alcohol in a ball mill for 4 hours and dry in air at 150 °C.

Mga kailangang kasangkapan:

Gilingang Bolang BakalGilingang Bolang Bakal
Etanol - antas laboratoryo, 95 %Etanol - antas laboratoryo, 95 %
Hurnong pantuyoHurnong pantuyo
3

Presinter in air at 1000 °C for 2 hours

Fire in air at 1000 °C for 2 hours.

Mga kailangang kasangkapan:

Muffle furnaceMuffle furnace
Krisol na may takip (porselana)Krisol na may takip (porselana)
Sipit ng KrisolSipit ng Krisol
Guwantes na Matibay sa InitGuwantes na Matibay sa Init
4

Mill again 4 hours, dry, form

Grind again with alcohol for 4 hours and dry. Example 19 extrudes a rod; ours: press discs at 1.5 tonnes per cm², as Example 18 moulds its rod.

Mga kailangang kasangkapan:

Gilingang Bolang BakalGilingang Bolang Bakal
Etanol - antas laboratoryo, 95 %Etanol - antas laboratoryo, 95 %
Hurnong pantuyoHurnong pantuyo
Haydroliko na pandiinHaydroliko na pandiin
Hulmahan sa pagpindot ng diskHulmahan sa pagpindot ng disk
5

Pass through a 1330 °C zone in 10 minutes

Sinter at 1330 °C by passing the pieces through a 10 cm hot zone at 10 mm per minute: 10 minutes in the heat.

Mga kailangang kasangkapan:

Hurnong TuboHurnong Tubo
Guwantes na Matibay sa InitGuwantes na Matibay sa Init
6

Magnetise the discs

The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.

Mga kailangang kasangkapan:

ElektromagnetoElektromagneto
KompasKompas

Mga Materyales

3

Mga Kinakailangang Kasangkapan

15

Ang blueprint na ito ay gumagawa ng

Kaugnay na Blueprint

Ang mga blueprint na ito ay nagbabahagi ng kaalaman — mga teknik, materyales, o prinsipyo

CC0 Pampublikong Domain

Ang blueprint na ito ay inilabas sa ilalim ng CC0. Malaya kang kumopya, magbago, mamahagi, at gumamit nang walang pahintulot.

Suportahan ang Maker sa pamamagitan ng pagbili ng mga produkto sa kanilang Blueprint Komisyon ng Maker itinakda ng mga Vendor, o lumikha ng bagong bersyon ng Blueprint na ito at isama bilang koneksyon sa iyong Blueprint upang ibahagi ang kita.

Talakayan

(0)

Mag-login upang sumali sa talakayan

Naglo-load ng mga komento...