Barium-Calcium Ferrite Disc Magnet: Part of the Barium Replaced by Calcium (Went, Philips 1956, Ex. 21)
Charlie

Nilikha ni

Charlie

28. Oktubre 2026DE
4
0
0
0
0

Barium-Calcium Ferrite Disc Magnet: Part of the Barium Replaced by Calcium (Went, Philips 1956, Ex. 21)

A ceramic magnet in which part of the barium is replaced by calcium: 0.06 mol barium carbonate and 0.04 mol calcium carbonate to 0.6 mol iron oxide, milled, fired in oxygen, milled again, pressed and passed quickly through a hot furnace. Went's rod held 1,660 gauss with a coercive force of 1,210 oersted. Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 21. They sintered rods; discs and the magnetising are ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Abantado
2 days

Mga Tagubilin

1

Weigh barium carbonate, chalk and iron oxide

Weigh 11.84 g barium carbonate (0.06 mol), 4.004 g calcium carbonate (0.04 mol) and 99.55 g ferric oxide (0.6 mol). Barium carbonate is poisonous if swallowed: gloves and a dust respirator.

Mga materyales para sa hakbang na ito:

Barium carbonate (witherite)Barium carbonate (witherite)11.84 g
Calcium carbonate (puting tisa)Calcium carbonate (puting tisa)4.004 g
Ferric oxideFerric oxide99.55 g

Mga kailangang kasangkapan:

Timbangang panimbangTimbangang panimbang
Gwantes na gomaGwantes na goma
Panala sa Hininga na P100Panala sa Hininga na P100
2

Mill with alcohol 4 hours and dry

Grind the mixture with alcohol in a ball mill for 4 hours, then dry it.

Mga kailangang kasangkapan:

Gilingang Bolang BakalGilingang Bolang Bakal
Etanol - antas laboratoryo, 95 %Etanol - antas laboratoryo, 95 %
Hurnong pantuyoHurnong pantuyo
3

Presinter in oxygen at 1000 °C for 2 hours

Fire the dry powder in oxygen at 1000 °C for 2 hours (ours: a tube furnace fed from an oxygen cylinder).

Mga kailangang kasangkapan:

Hurnong TuboHurnong Tubo
OksihenoOksiheno
Tangke ng gas na may presyonTangke ng gas na may presyon
Guwantes na Matibay sa InitGuwantes na Matibay sa Init
4

Mill again 4 hours, dry, press at 1.5 t/cm²

Grind with alcohol in the ball mill for 4 hours, dry, and press at 1.5 tonnes per cm² (ours: discs instead of rods).

Mga kailangang kasangkapan:

Gilingang Bolang BakalGilingang Bolang Bakal
Etanol - antas laboratoryo, 95 %Etanol - antas laboratoryo, 95 %
Hurnong pantuyoHurnong pantuyo
Haydroliko na pandiinHaydroliko na pandiin
Hulmahan sa pagpindot ng diskHulmahan sa pagpindot ng disk
5

Pass through a 1200 °C zone in 10 minutes

Sinter at 1200 °C by passing the pieces through a 10 cm hot zone at 10 mm per minute, which is 10 minutes in the heat.

Mga kailangang kasangkapan:

Hurnong TuboHurnong Tubo
Guwantes na Matibay sa InitGuwantes na Matibay sa Init
6

Magnetise the discs

The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.

Mga kailangang kasangkapan:

ElektromagnetoElektromagneto
KompasKompas

Mga Materyales

3

Mga Kinakailangang Kasangkapan

14

Ang blueprint na ito ay gumagawa ng

Kaugnay na Blueprint

Ang mga blueprint na ito ay nagbabahagi ng kaalaman — mga teknik, materyales, o prinsipyo

CC0 Pampublikong Domain

Ang blueprint na ito ay inilabas sa ilalim ng CC0. Malaya kang kumopya, magbago, mamahagi, at gumamit nang walang pahintulot.

Suportahan ang Maker sa pamamagitan ng pagbili ng mga produkto sa kanilang Blueprint Komisyon ng Maker itinakda ng mga Vendor, o lumikha ng bagong bersyon ng Blueprint na ito at isama bilang koneksyon sa iyong Blueprint upang ibahagi ang kita.

Talakayan

(0)

Mag-login upang sumali sa talakayan

Naglo-load ng mga komento...