Barium-Calcium Ferrite Disc Magnet: Equal Barium and Calcium, Sintered at 1280 °C (Went, Philips 1956, Ex. 22)
Charlie

Nilikha ni

Charlie

28. Oktubre 2026DE
5
0
0
0
0

Barium-Calcium Ferrite Disc Magnet: Equal Barium and Calcium, Sintered at 1280 °C (Went, Philips 1956, Ex. 22)

A ceramic magnet with equal parts barium and calcium: 0.3 mol barium carbonate, 0.3 mol calcium carbonate and 3.1 mol iron oxide, milled 15 hours, pressed and passed through a 1280 °C furnace in 10 minutes, with no presintering. Went's rod held 1,595 gauss with a coercive force of 1,890 oersted. Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 22. They sintered rods; discs and the magnetising are ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Abantado
2 days

Mga Tagubilin

1

Weigh barium carbonate, chalk and iron oxide

Weigh 59.5 g barium carbonate (0.3 mol), 30.2 g calcium carbonate (0.3 mol) and 500.0 g ferric oxide (3.1 mol). Barium carbonate is poisonous if swallowed: gloves and a dust respirator.

Mga materyales para sa hakbang na ito:

Barium carbonate (witherite)Barium carbonate (witherite)59.5 g
Calcium carbonate (puting tisa)Calcium carbonate (puting tisa)30.2 g
Ferric oxideFerric oxide500 g

Mga kailangang kasangkapan:

Timbangang panimbangTimbangang panimbang
Gwantes na gomaGwantes na goma
Panala sa Hininga na P100Panala sa Hininga na P100
2

Mill with alcohol 15 hours, dry, press

Grind with alcohol in a ball mill for 15 hours, dry, and press at 1.5 tonnes per cm² (ours: discs instead of rods). No presintering.

Mga kailangang kasangkapan:

Gilingang Bolang BakalGilingang Bolang Bakal
Etanol - antas laboratoryo, 95 %Etanol - antas laboratoryo, 95 %
Hurnong pantuyoHurnong pantuyo
Haydroliko na pandiinHaydroliko na pandiin
Hulmahan sa pagpindot ng diskHulmahan sa pagpindot ng disk
3

Pass through a 1280 °C zone in 10 minutes

Sinter at 1280 °C by passing the pieces through a 10 cm hot zone at 10 mm per minute: 10 minutes in the heat.

Mga kailangang kasangkapan:

Hurnong TuboHurnong Tubo
Guwantes na Matibay sa InitGuwantes na Matibay sa Init
4

Magnetise the discs

The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.

Mga kailangang kasangkapan:

ElektromagnetoElektromagneto
KompasKompas

Mga Materyales

3

Mga Kinakailangang Kasangkapan

12

Ang blueprint na ito ay gumagawa ng

Kaugnay na Blueprint

Ang mga blueprint na ito ay nagbabahagi ng kaalaman — mga teknik, materyales, o prinsipyo

CC0 Pampublikong Domain

Ang blueprint na ito ay inilabas sa ilalim ng CC0. Malaya kang kumopya, magbago, mamahagi, at gumamit nang walang pahintulot.

Suportahan ang Maker sa pamamagitan ng pagbili ng mga produkto sa kanilang Blueprint Komisyon ng Maker itinakda ng mga Vendor, o lumikha ng bagong bersyon ng Blueprint na ito at isama bilang koneksyon sa iyong Blueprint upang ibahagi ang kita.

Talakayan

(0)

Mag-login upang sumali sa talakayan

Naglo-load ng mga komento...