Barium Ferrite Disc Magnet: 1 mol BaCO3 to 3.5 mol Iron Oxide, 1330 °C (Went, Philips 1956, Ex. 3)
A barium ferrite with more iron oxide: 1 mol barium carbonate to 3.5 mol, made as in Example 1 and passed through a 1330 °C furnace in 20 minutes. Went's rod held 1,600 gauss with a coercive force of 1,990 oersted.
Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 3. They sintered rods; discs and the magnetising are ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Abantado
2 days
Mga Tagubilin
1
1
Weigh barium carbonate and iron oxide
Weigh barium carbonate and iron oxide
Weigh 201.1 g barium carbonate (1 mol) and 560.7 g ferric oxide (3.5 mol). Barium carbonate is poisonous if swallowed: gloves and a dust respirator.
Mga materyales para sa hakbang na ito:
Barium carbonate (witherite)201.1 g
Ferric oxide560.7 gMga kailangang kasangkapan:
Timbangang panimbang
Gwantes na goma
Panala sa Hininga na P1002
2
Mill with alcohol 13.5 hours, dry and sieve
Mill with alcohol 13.5 hours, dry and sieve
Grind the mixture with alcohol in a ball mill for 13.5 hours, then dry it and sieve it.
Mga kailangang kasangkapan:
Gilingang Bolang Bakal
Etanol - antas laboratoryo, 95 %
Hurnong pantuyo
Bithay3
3
Knead with a binder and form
Knead with a binder and form
Mix 300 g of the powder with a binder such as polyvinyl alcohol (Went names it or nitrocellulose) into a kneadable mass. The patent extrudes rods about 3 mm across; ours: press discs at 1.5 tonnes per cm², as in its other examples. Dry them in air for about 24 hours.
Mga kailangang kasangkapan:
Pulbos na polyvinyl alcohol
Haydroliko na pandiin
Hulmahan sa pagpindot ng disk
Hurnong pantuyo4
4
Pass through a 1330 °C zone in 20 minutes
Pass through a 1330 °C zone in 20 minutes
Sinter in air at 1330 °C by passing the pieces through a 10 cm hot zone at 5 mm per minute: 20 minutes in the heat.
Mga kailangang kasangkapan:
Hurnong Tubo
Guwantes na Matibay sa Init5
5
Magnetise the discs
Magnetise the discs
The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.
Mga kailangang kasangkapan:
Elektromagneto
KompasMga Materyales
2- 201.1 gPlaceholder
- 560.7 gPlaceholder
Mga Kinakailangang Kasangkapan
14- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
Ang blueprint na ito ay gumagawa ng
Kaugnay na Blueprint
Ang mga blueprint na ito ay nagbabahagi ng kaalaman — mga teknik, materyales, o prinsipyo
CC0 Pampublikong Domain
Ang blueprint na ito ay inilabas sa ilalim ng CC0. Malaya kang kumopya, magbago, mamahagi, at gumamit nang walang pahintulot.
Suportahan ang Maker sa pamamagitan ng pagbili ng mga produkto sa kanilang Blueprint Komisyon ng Maker itinakda ng mga Vendor, o lumikha ng bagong bersyon ng Blueprint na ito at isama bilang koneksyon sa iyong Blueprint upang ibahagi ang kita.