Barium Ferrite Disc Magnet from Natural Magnetite, Presintered at 900 °C (Went, Philips 1956, Ex. 36, Procedure 1)
A barium ferrite magnet made from natural magnetite instead of ferric oxide: barium carbonate and magnetite ground 18 hours, presintered 3 hours at 900 °C, ground again 18 hours, pressed and sintered 2 hours at 1200 °C. Went's rod held 1,450 gauss with a coercive force of 2,425 oersted.
Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 36. They sintered rods; discs and the magnetising are ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Abantado
2 days
Mga Tagubilin
1
1
Weigh barium carbonate and magnetite
Weigh barium carbonate and magnetite
Weigh 9.9 g barium carbonate (0.05 mol) and 46.9 g natural magnetite, Fe3O4 (0.20 mol). Barium carbonate is poisonous if swallowed: gloves and a dust respirator.
Mga materyales para sa hakbang na ito:
Barium carbonate (witherite)9.9 g
Magnetite46.9 gMga kailangang kasangkapan:
Timbangang panimbang
Gwantes na goma
Panala sa Hininga na P1002
2
Grind 18 hours in a ball mill
Grind 18 hours in a ball mill
Grind the mixture in a ball mill for 18 hours. The patent does not say whether wet or dry.
Mga kailangang kasangkapan:
Gilingang Bolang Bakal
Panala sa Hininga na P1003
3
Presinter at 900 °C for 3 hours
Presinter at 900 °C for 3 hours
Fire the ground mixture at 900 °C for three hours and let it cool.
Mga kailangang kasangkapan:
Muffle furnace
Krisol na may takip (porselana)
Sipit ng Krisol
Guwantes na Matibay sa Init4
4
Grind 18 hours in a ball mill
Grind 18 hours in a ball mill
Grind it again in a ball mill for 18 hours. The patent does not say whether wet or dry.
Mga kailangang kasangkapan:
Gilingang Bolang Bakal
Panala sa Hininga na P1005
5
Press at 1.5 t/cm²
Press at 1.5 t/cm²
Press at 1.5 tonnes per cm² (ours: discs instead of a rod).
Mga kailangang kasangkapan:
Haydroliko na pandiin
Hulmahan sa pagpindot ng disk6
6
Sinter at 1200 °C for 2 hours
Sinter at 1200 °C for 2 hours
Sinter at 1200 °C for 2 hours. The patent gives no atmosphere for this example. Went's rod: 1,450 gauss, 2,425 oersted.
Mga kailangang kasangkapan:
Muffle furnace
Sipit ng Krisol
Guwantes na Matibay sa Init7
7
Magnetise the discs
Magnetise the discs
The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.
Mga kailangang kasangkapan:
Elektromagneto
KompasMga Kinakailangang Kasangkapan
12- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
Ang blueprint na ito ay gumagawa ng
Kaugnay na Blueprint
Ang mga blueprint na ito ay nagbabahagi ng kaalaman — mga teknik, materyales, o prinsipyo
CC0 Pampublikong Domain
Ang blueprint na ito ay inilabas sa ilalim ng CC0. Malaya kang kumopya, magbago, mamahagi, at gumamit nang walang pahintulot.
Suportahan ang Maker sa pamamagitan ng pagbili ng mga produkto sa kanilang Blueprint Komisyon ng Maker itinakda ng mga Vendor, o lumikha ng bagong bersyon ng Blueprint na ito at isama bilang koneksyon sa iyong Blueprint upang ibahagi ang kita.