Barium Ferrite Disc Magnet: 0.4 mol BaCO3 to 3.7 mol Iron Oxide, 1330 °C (Went, Philips 1956, Ex. 6)
Charlie

Nilikha ni

Charlie

28. Oktubre 2026DE
8
0
0
0
0

Barium Ferrite Disc Magnet: 0.4 mol BaCO3 to 3.7 mol Iron Oxide, 1330 °C (Went, Philips 1956, Ex. 6)

A barium ferrite with 0.4 mol barium carbonate to 3.7 mol iron oxide, made as in Example 4 and passed through a 1330 °C furnace in 20 minutes. Went's rod held 1,200 gauss with a coercive force of 1,950 oersted. Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 6. They sintered rods; discs and the magnetising are ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Abantado
2 days

Mga Tagubilin

1

Weigh barium carbonate and iron oxide

Weigh 79.4 g barium carbonate (0.4 mol) and 580.9 g ferric oxide (3.7 mol). Barium carbonate is poisonous if swallowed: gloves and a dust respirator.

Mga materyales para sa hakbang na ito:

Barium carbonate (witherite)Barium carbonate (witherite)79.4 g
Ferric oxideFerric oxide580.9 g

Mga kailangang kasangkapan:

Timbangang panimbangTimbangang panimbang
Gwantes na gomaGwantes na goma
Panala sa Hininga na P100Panala sa Hininga na P100
2

Mill with alcohol 15.5 hours, dry and sieve

As in Example 4: grind the mixture with alcohol in a ball mill for 15.5 hours, then dry it and sieve it.

Mga kailangang kasangkapan:

Gilingang Bolang BakalGilingang Bolang Bakal
Etanol - antas laboratoryo, 95 %Etanol - antas laboratoryo, 95 %
Hurnong pantuyoHurnong pantuyo
BithayBithay
3

Knead with a binder and form

Mix 300 g of the powder with a binder such as polyvinyl alcohol (Went names it or nitrocellulose) into a kneadable mass. The patent extrudes rods about 3 mm across; ours: press discs at 1.5 tonnes per cm², as in its other examples. Dry them in air for about 24 hours.

Mga kailangang kasangkapan:

Pulbos na polyvinyl alcoholPulbos na polyvinyl alcohol
Haydroliko na pandiinHaydroliko na pandiin
Hulmahan sa pagpindot ng diskHulmahan sa pagpindot ng disk
Hurnong pantuyoHurnong pantuyo
4

Pass through a 1330 °C zone in 20 minutes

Sinter in air at 1330 °C by passing the pieces through a 10 cm hot zone at 5 mm per minute: 20 minutes in the heat.

Mga kailangang kasangkapan:

Hurnong TuboHurnong Tubo
Guwantes na Matibay sa InitGuwantes na Matibay sa Init
5

Magnetise the discs

The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.

Mga kailangang kasangkapan:

ElektromagnetoElektromagneto
KompasKompas

Mga Materyales

2

Mga Kinakailangang Kasangkapan

14

Ang blueprint na ito ay gumagawa ng

Kaugnay na Blueprint

Ang mga blueprint na ito ay nagbabahagi ng kaalaman — mga teknik, materyales, o prinsipyo

CC0 Pampublikong Domain

Ang blueprint na ito ay inilabas sa ilalim ng CC0. Malaya kang kumopya, magbago, mamahagi, at gumamit nang walang pahintulot.

Suportahan ang Maker sa pamamagitan ng pagbili ng mga produkto sa kanilang Blueprint Komisyon ng Maker itinakda ng mga Vendor, o lumikha ng bagong bersyon ng Blueprint na ito at isama bilang koneksyon sa iyong Blueprint upang ibahagi ang kita.

Talakayan

(0)

Mag-login upang sumali sa talakayan

Naglo-load ng mga komento...