Barium-Strontium Ferrite Disc Magnet: 0.09 mol BaCO3, 0.21 mol SrCO3, 1300 °C (Went, Philips 1956, Ex. 31)
Charlie

Nilikha ni

Charlie

28. Oktubre 2026DE
6
0
0
0
0

Barium-Strontium Ferrite Disc Magnet: 0.09 mol BaCO3, 0.21 mol SrCO3, 1300 °C (Went, Philips 1956, Ex. 31)

A ceramic magnet with both barium and strontium: 0.09 mol barium carbonate and 0.21 mol strontium carbonate to 2.7 mol iron oxide, milled as in Example 28, pressed and passed through a 1300 °C furnace in 10 minutes. Went's rod held 1,340 gauss with a coercive force of 2,640 oersted. Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 31. They sintered rods; discs and the magnetising are ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Abantado
2 days

Mga Tagubilin

1

Weigh the carbonates and iron oxide

Weigh 17.9 g barium carbonate (0.09 mol), 31.0 g strontium carbonate (0.21 mol), 435.5 g ferric oxide (2.7 mol). Barium carbonate is poisonous if swallowed: gloves and a dust respirator.

Mga materyales para sa hakbang na ito:

Barium carbonate (witherite)Barium carbonate (witherite)17.9 g
Strontium carbonateStrontium carbonate31 g
Ferric oxideFerric oxide435.5 g

Mga kailangang kasangkapan:

Timbangang panimbangTimbangang panimbang
Gwantes na gomaGwantes na goma
Panala sa Hininga na P100Panala sa Hininga na P100
2

Mill with alcohol 15 hours, dry

As in Example 28: grind the mixture with alcohol in a ball mill for 15 hours, then dry it.

Mga kailangang kasangkapan:

Gilingang Bolang BakalGilingang Bolang Bakal
Etanol - antas laboratoryo, 95 %Etanol - antas laboratoryo, 95 %
Hurnong pantuyoHurnong pantuyo
3

Press the powder

Example 28 moulds a rod without giving the pressure. Ours: press discs at 1.5 tonnes per cm², the pressure of the patent's other examples.

Mga kailangang kasangkapan:

Haydroliko na pandiinHaydroliko na pandiin
Hulmahan sa pagpindot ng diskHulmahan sa pagpindot ng disk
4

Pass through a 1300 °C zone in 10 minutes

Sinter in air at 1300 °C by passing the pieces through a 10 cm hot zone at 10 mm per minute: 10 minutes in the heat.

Mga kailangang kasangkapan:

Hurnong TuboHurnong Tubo
Guwantes na Matibay sa InitGuwantes na Matibay sa Init
5

Magnetise the discs

The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.

Mga kailangang kasangkapan:

ElektromagnetoElektromagneto
KompasKompas

Mga Materyales

3

Mga Kinakailangang Kasangkapan

12

Ang blueprint na ito ay gumagawa ng

CC0 Pampublikong Domain

Ang blueprint na ito ay inilabas sa ilalim ng CC0. Malaya kang kumopya, magbago, mamahagi, at gumamit nang walang pahintulot.

Suportahan ang Maker sa pamamagitan ng pagbili ng mga produkto sa kanilang Blueprint Komisyon ng Maker itinakda ng mga Vendor, o lumikha ng bagong bersyon ng Blueprint na ito at isama bilang koneksyon sa iyong Blueprint upang ibahagi ang kita.

Talakayan

(0)

Mag-login upang sumali sa talakayan

Naglo-load ng mga komento...