Ceramic Disc Capacitors: Barium Titanate with Nickel Stannate, Pressed, Fired and Silvered (Coffeen, US 2,789,061)
Ed

Nilikha ni

Ed

2. Nobyembre 2026FI
10
0
0
0
0

Ceramic Disc Capacitors: Barium Titanate with Nickel Stannate, Pressed, Fired and Silvered (Coffeen, US 2,789,061)

Barium titanate with 3 mole % nickel stannate is calcined, pressed into small discs and fired hard. Silver is fired onto both faces and a lead soldered to each, giving ceramic disc capacitors of high capacity for their size. Result: discs 3/8 inch across and about 1/10 inch thick with a dielectric constant averaging 2380 and a dissipation factor of 0.58 %. Between 25 and 85 °C the dielectric constant rose at most 17 % and fell at most 7 %. Source: W. W. Coffeen (Metal & Thermit Corp.), US 2,789,061 (1957). Unknown: how the barium titanate, the nickel stannate and the tinned lead wire are made; the patent uses them ready-made. Picture: Wikimedia Commons.
Abantado
10 days

Mga Tagubilin

1

Weigh and slurry

Weigh 19.32 g of barium titanate and 0.68 g of hydrated nickel stannate (about NiSnO3·2H2O), which is 97 mole % BaTiO3 and 3 mole % NiSnO3. Slurry them with 50 cc of distilled water. The patent prefers 2 to 4 mole % nickel stannate; 1 to 15 % works.

Mga materyales para sa hakbang na ito:

Barium titanateBarium titanate19.32 g
Nickel stannateNickel stannate0.68 g

Mga kailangang kasangkapan:

Distiladong TubigDistiladong Tubig
Tumpak na Digital na TimbanganTumpak na Digital na Timbangan
Platong PansingawPlatong Pansingaw
2

Dry, sieve and calcine

Dry the slurry, crush it to pass a 50 mesh screen, moisten it with 5 % of a 2 1/2 % starch solution and press it into one slug. Calcine the slug for one hour at 1600 °F (871 °C). Ours: potato starch, a drying oven, mortar and pestle.

Mga kailangang kasangkapan:

Almirol ng patatasAlmirol ng patatas
Hurnong pantuyoHurnong pantuyo
Almires at PanghaloAlmires at Panghalo
BithayBithay
Haydroliko na pandiinHaydroliko na pandiin
Hurnong mataas ang initHurnong mataas ang init
3

Press the discs

Grind the calcine to pass a 325 mesh screen, moisten it again with starch solution, and press small discs 3/8 inch in diameter and about 1/10 inch thick at 20,000 pounds per square inch.

Mga kailangang kasangkapan:

Almires at PanghaloAlmires at Panghalo
Bistay na Pinong LambatBistay na Pinong Lambat
Almirol ng patatasAlmirol ng patatas
Haydroliko na pandiinHaydroliko na pandiin
Hulmahan sa pagpindot ng diskHulmahan sa pagpindot ng disk
4

Fire on platinum

Fire the discs on platinum foil at 2400 °F (1316 °C) for one hour. They come out with zero absorption.

Mga kailangang kasangkapan:

Hurnong mataas ang initHurnong mataas ang init
PlatinoPlatino
5

Silver and lead

Paint silver paint on both faces and fire the discs at 1350 °F (732 °C) for one hour. Solder tinned copper lead wires directly to the silver electrodes. Age at least a week before measuring. Ours: a fine brush and a soldering iron.

Mga materyales para sa hakbang na ito:

Pinapasong pinturang pilakPinapasong pinturang pilak1 both faces
Tinned copper wireTinned copper wire2 leads per disc
Kawad na PanghinangKawad na Panghinang1 a little

Mga kailangang kasangkapan:

Mga pinsel na pinong ang duloMga pinsel na pinong ang dulo
Hurnong mataas ang initHurnong mataas ang init
PanghinangPanghinang

Mga Materyales

5

Mga Kinakailangang Kasangkapan

14

Ang blueprint na ito ay gumagawa ng

CC0 Pampublikong Domain

Ang blueprint na ito ay inilabas sa ilalim ng CC0. Malaya kang kumopya, magbago, mamahagi, at gumamit nang walang pahintulot.

Suportahan ang Maker sa pamamagitan ng pagbili ng mga produkto sa kanilang Blueprint Komisyon ng Maker itinakda ng mga Vendor, o lumikha ng bagong bersyon ng Blueprint na ito at isama bilang koneksyon sa iyong Blueprint upang ibahagi ang kita.

Talakayan

(0)

Mag-login upang sumali sa talakayan

Naglo-load ng mga komento...