E-glass Fibre Strand: Alkali-Free Lime-Alumina-Borosilicate Glass Drawn to Filament

Fibre from ordinary glass carries alkali on its huge surface; it takes up water from the air and slowly destroys itself, and it conducts electricity. Schoenlaub's Owens-Corning glass (US 2,334,961, 1943) has no alkali at all: lime, magnesia, alumina and silica fluxed with boric oxide. It was made to be drawn into fibres for insulation and textiles. It is melted at up to 1420 °C and drawn into continuous filaments on a fast spool. The picture: our diagram.
Abantado
2 days

Mga Tagubilin

1

Weigh out the batch

The patent's example glass: lime (CaO) 17.5 %, magnesia (MgO) 4.5 %, alumina 14.0 %, silica 54.0 %, boric oxide 10.0 %. Ours: weigh those five oxides in those proportions and mix them. Keep within the patent's limits; small changes make this glass devitrify.

Mga materyales para sa hakbang na ito:

Apog na hindi pa napapatayApog na hindi pa napapatay17.5 parts
Oksido ng magnesiyoOksido ng magnesiyo4.5 parts
Pulbos na alumina (aluminum oxide)Pulbos na alumina (aluminum oxide)14 parts
Buhangin ng KuwarsoBuhangin ng Kuwarso54 parts
Oksidong borikoOksidong boriko10 parts

Mga kailangang kasangkapan:

Timbangang panimbangTimbangang panimbang
Salaming pangkaligtasanSalaming pangkaligtasan
2

Melt at no more than 1420 °C

Melt the batch in a glass tank furnace without going above 1420 °C; the patent's day tanks ran on a 24-hour cycle.

Mga kailangang kasangkapan:

Hurno sa pagtunaw ng salaminHurno sa pagtunaw ng salamin
PirometroPirometro
Guwantes na Matibay sa InitGuwantes na Matibay sa Init
Salaming pangkaligtasanSalaming pangkaligtasan
3

Feed the platinum bushing

Draw from a platinum-rhodium bushing like Slayter and Thomas's, heated by an adjustable current. The drawing range of this glass is about 2000–2400 °F (1090–1320 °C). A blower below the nozzles sets each filament.

Mga kailangang kasangkapan:

Kahon na Platinum-RhodiumKahon na Platinum-Rhodium
Step-Down TransformerStep-Down Transformer
PirometroPirometro
Panghihip ng hanginPanghihip ng hangin
Guwantes na Matibay sa InitGuwantes na Matibay sa Init
4

Wind on a fast spool

Gather the filaments into a strand and wind it on a spool running as fast as 6,000–10,000 ft per minute (30–50 m/s). Filaments come out about .0001–.0003 in (2.5–7.6 µm) thick. The strand can then be twisted and plied into yarn.

Mga kailangang kasangkapan:

Tambol na Pambalot ng HiblaTambol na Pambalot ng Hibla

Mga Materyales

5

Mga Kinakailangang Kasangkapan

9

Ang blueprint na ito ay gumagawa ng

Kaugnay na Blueprint

Ang mga blueprint na ito ay nagbabahagi ng kaalaman — mga teknik, materyales, o prinsipyo

CC0 Pampublikong Domain

Ang blueprint na ito ay inilabas sa ilalim ng CC0. Malaya kang kumopya, magbago, mamahagi, at gumamit nang walang pahintulot.

Suportahan ang Maker sa pamamagitan ng pagbili ng mga produkto sa kanilang Blueprint Komisyon ng Maker itinakda ng mga Vendor, o lumikha ng bagong bersyon ng Blueprint na ito at isama bilang koneksyon sa iyong Blueprint upang ibahagi ang kita.

Talakayan

(0)

Mag-login upang sumali sa talakayan

Naglo-load ng mga komento...