Extruded Polystyrene Foam: Butylene-Blown Logs 20 Inches Across (McIntire, Dow 1948, Ex. 4)

Extruded polystyrene foam blown with a butylene gas fraction. 300 lb of polystyrene and about 130 lb of the fraction stand two days at 110 °C under 265 psi. Opened again and again, the tower let out foam logs 20 inches across and 20 feet long, weighing only 0.8 lb per cubic foot. Unknown: a source for the butylene fraction, linked to an unknown head. Source: O. R. McIntire (Dow), US 2,450,436 (1948), Example 4. Picture: the patent's drawing.
Abantado
3 days

Mga Tagubilin

1

Charge the tower with polystyrene

Charge a high-pressure tower with 300 lb of granular polystyrene.

Mga materyales para sa hakbang na ito:

PolistirenaPolistirena300 libra

Mga kailangang kasangkapan:

Reactor na may presyonReactor na may presyon
Timbangang panimbangTimbangang panimbang
Gwantes na gomaGwantes na goma
2

Add the butylene fraction

Add about 130 lb of a cracked-oil gas fraction that is about 87 % normal butylenes, with some butanes and butadiene, under pressure. Unknown: a source for this fraction. Flammable gas: no flames, strong ventilation.

Mga materyales para sa hakbang na ito:

Bahagi ng cracked gas na butyleneBahagi ng cracked gas na butylene130 libra

Mga kailangang kasangkapan:

Tangke ng gas na may presyonTangke ng gas na may presyon
Reactor na may presyonReactor na may presyon
Salamin Laban sa Tilamsik ng KemikalSalamin Laban sa Tilamsik ng Kemikal
3

Heat two days at 110 °C

Close the tower and heat it at 110 °C for two days. The gauge pressure stays at 265 psi.

Mga kailangang kasangkapan:

Reactor na may presyonReactor na may presyon
Termometrong PanlaboratoryoTermometrong Panlaboratoryo
4

Let out logs through a 3.25 inch outlet

Open and close the 3.25 inch outlet near the bottom again and again. Each portion swells into a foam log 20 inches across and about 20 feet long, with fine, even, closed cells, weighing 0.8 lb per cubic foot.

Mga kailangang kasangkapan:

Reactor na may presyonReactor na may presyon
Salamin Laban sa Tilamsik ng KemikalSalamin Laban sa Tilamsik ng Kemikal
Gwantes na gomaGwantes na goma
5

Saw into boards

When the foam has set, saw it lengthwise into slabs (ours: a woodworking saw).

Mga kailangang kasangkapan:

Lagaring pangkarpinteroLagaring pangkarpintero
Gwantes na gomaGwantes na goma

Mga Materyales

2

Mga Kinakailangang Kasangkapan

7

Kaugnay na Blueprint

Ang mga blueprint na ito ay nagbabahagi ng kaalaman — mga teknik, materyales, o prinsipyo

CC0 Pampublikong Domain

Ang blueprint na ito ay inilabas sa ilalim ng CC0. Malaya kang kumopya, magbago, mamahagi, at gumamit nang walang pahintulot.

Suportahan ang Maker sa pamamagitan ng pagbili ng mga produkto sa kanilang Blueprint Komisyon ng Maker itinakda ng mga Vendor, o lumikha ng bagong bersyon ng Blueprint na ito at isama bilang koneksyon sa iyong Blueprint upang ibahagi ang kita.

Talakayan

(0)

Mag-login upang sumali sa talakayan

Naglo-load ng mga komento...