Extruded Polystyrene Foam: Propylene-Blown Log Let Out at 50 °C (McIntire, Dow 1948, Ex. 3, Test 2)
Charlie

Nilikha ni

Charlie

28. Oktubre 2026DE
8
0
0
0
0

Extruded Polystyrene Foam: Propylene-Blown Log Let Out at 50 °C (McIntire, Dow 1948, Ex. 3, Test 2)

Extruded polystyrene foam blown with a propylene gas fraction instead of methyl chloride. Polystyrene stands two days at 40 °C with the propylene under pressure and becomes a gel. Let out at 50 °C (250 psi in the tower), it swelled into a log 6 to 9 inches across, weighing 4.8 lb per cubic foot, with somewhat smaller, uniform cells. Source: O. R. McIntire (Dow), US 2,450,436 (1948), Example 3. Picture: the patent's drawing.
Abantado
3 days

Mga Tagubilin

1

Charge the tower with polystyrene

Charge a high-pressure tower with 300 lb of granular polystyrene.

Mga materyales para sa hakbang na ito:

PolistirenaPolistirena300 libra

Mga kailangang kasangkapan:

Reactor na may presyonReactor na may presyon
Timbangang panimbangTimbangang panimbang
Gwantes na gomaGwantes na goma
2

Add the propylene fraction

Add 100 lb of a cracked-oil gas fraction that is about 93 % propylene, under pressure, and close the tower. Propylene is a flammable gas: no flames, strong ventilation.

Mga materyales para sa hakbang na ito:

PropylenePropylene100 libra

Mga kailangang kasangkapan:

Tangke ng gas na may presyonTangke ng gas na may presyon
Reactor na may presyonReactor na may presyon
Salamin Laban sa Tilamsik ng KemikalSalamin Laban sa Tilamsik ng Kemikal
3

Stand two days at 40 °C

Let the tower stand for two days at 40 °C while the polystyrene takes up the propylene.

Mga kailangang kasangkapan:

Reactor na may presyonReactor na may presyon
Termometrong PanlaboratoryoTermometrong Panlaboratoryo
4

Let it out at 50 °C

Open the valved outlet near the bottom (3.25 inch in the patent) at 50 °C. The pressure is about 250 psi. The gel flows out and swells into a log 6 to 9 inches across, 4.8 lb per cubic foot, with somewhat smaller, uniform cells. Close the outlet again. The patent heated step by step (50, 60, 75 °C) for several hours each, letting a portion out at each step.

Mga kailangang kasangkapan:

Reactor na may presyonReactor na may presyon
Termometrong PanlaboratoryoTermometrong Panlaboratoryo
Salamin Laban sa Tilamsik ng KemikalSalamin Laban sa Tilamsik ng Kemikal
Gwantes na gomaGwantes na goma
5

Saw into boards

When the foam has set, saw it lengthwise into slabs (ours: a woodworking saw).

Mga kailangang kasangkapan:

Lagaring pangkarpinteroLagaring pangkarpintero
Gwantes na gomaGwantes na goma

Mga Materyales

2
  • 300 libra
    Placeholder
  • 100 libra
    Placeholder

Mga Kinakailangang Kasangkapan

7

CC0 Pampublikong Domain

Ang blueprint na ito ay inilabas sa ilalim ng CC0. Malaya kang kumopya, magbago, mamahagi, at gumamit nang walang pahintulot.