Extruded Polystyrene Foam: Propylene-Blown Log Let Out at 75 °C (McIntire, Dow 1948, Ex. 3, Test 4)
Extruded polystyrene foam blown with a propylene gas fraction instead of methyl chloride. Polystyrene stands two days at 40 °C with the propylene under pressure and becomes a gel. Let out at 75 °C (395 psi in the tower), it swelled into a log 18 to 20 inches across, weighing 2.9 lb per cubic foot, with uniform cells finer than at 60 °C.
Source: O. R. McIntire (Dow), US 2,450,436 (1948), Example 3. Picture: the patent's drawing.
Abantado
3 days
Mga Tagubilin
1
1
Charge the tower with polystyrene
Charge the tower with polystyrene
Charge a high-pressure tower with 300 lb of granular polystyrene.
Mga materyales para sa hakbang na ito:
Polistirena300 libraMga kailangang kasangkapan:
Reactor na may presyon
Timbangang panimbang
Gwantes na goma2
2
Add the propylene fraction
Add the propylene fraction
Add 100 lb of a cracked-oil gas fraction that is about 93 % propylene, under pressure, and close the tower. Propylene is a flammable gas: no flames, strong ventilation.
Mga materyales para sa hakbang na ito:
Propylene100 libraMga kailangang kasangkapan:
Tangke ng gas na may presyon
Reactor na may presyon
Salamin Laban sa Tilamsik ng Kemikal3
3
Stand two days at 40 °C
Stand two days at 40 °C
Let the tower stand for two days at 40 °C while the polystyrene takes up the propylene.
Mga kailangang kasangkapan:
Reactor na may presyon
Termometrong Panlaboratoryo4
4
Let it out at 75 °C
Let it out at 75 °C
Open the valved outlet near the bottom (3.25 inch in the patent) at 75 °C. The pressure is about 395 psi. The gel flows out and swells into a log 18 to 20 inches across, 2.9 lb per cubic foot, with uniform cells finer than at 60 °C. Close the outlet again. The patent heated step by step (50, 60, 75 °C) for several hours each, letting a portion out at each step.
Mga kailangang kasangkapan:
Reactor na may presyon
Termometrong Panlaboratoryo
Salamin Laban sa Tilamsik ng Kemikal
Gwantes na goma5
5
Saw into boards
Saw into boards
When the foam has set, saw it lengthwise into slabs (ours: a woodworking saw).
Mga kailangang kasangkapan:
Lagaring pangkarpintero
Gwantes na gomaMga Kinakailangang Kasangkapan
7- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
Ang blueprint na ito ay gumagawa ng
Kaugnay na Blueprint
Ang mga blueprint na ito ay nagbabahagi ng kaalaman — mga teknik, materyales, o prinsipyo
CC0 Pampublikong Domain
Ang blueprint na ito ay inilabas sa ilalim ng CC0. Malaya kang kumopya, magbago, mamahagi, at gumamit nang walang pahintulot.
Suportahan ang Maker sa pamamagitan ng pagbili ng mga produkto sa kanilang Blueprint Komisyon ng Maker itinakda ng mga Vendor, o lumikha ng bagong bersyon ng Blueprint na ito at isama bilang koneksyon sa iyong Blueprint upang ibahagi ang kita.