Ferrite Toroid Core: Copper-Zinc Ferrite Fired at 1050 °C, Held at 600 °C in Oxygen (Snoek)
Charlie

Nilikha ni

Charlie

21. Oktubre 2026DE
16
0
0
0
0

Ferrite Toroid Core: Copper-Zinc Ferrite Fired at 1050 °C, Held at 600 °C in Oxygen (Snoek)

Ferrite is a ceramic magnet: iron oxide combined with other metal oxides, carrying magnetic flux while hardly conducting electricity. Snoek at Philips (US 2,452,531, 1948) made this copper-zinc ferrite ring at a lower heat: technical copper oxide, zinc oxide and iron oxide with 1 % brownstone, fired at 1050 °C, then held 14 hours at 600 °C, all in oxygen. His ring had an initial permeability of 385. The picture: our diagram.
Abantado
2 days

Mga Tagubilin

1

Mix 20.7 : 31.6 : 47.7 mol + 1 % brownstone

Mix technical copper oxide, zinc oxide and iron oxide in the molecular ratio 20.7 : 31.6 : 47.7 (on the pure oxides) and add 1 % by weight of brownstone (manganese dioxide). Ours, by weight: 13.91 g copper oxide, 21.73 g zinc oxide and 64.36 g ferric oxide per 100 g, plus 1 g brownstone.

Mga materyales para sa hakbang na ito:

Copper OxideCopper Oxide13.91 g
Pulbos ng Zinc OxidePulbos ng Zinc Oxide21.73 g
Ferric oxideFerric oxide64.36 g
Manganese dioxide (pirolusita)Manganese dioxide (pirolusita)1 g

Mga kailangang kasangkapan:

Timbangang panimbangTimbangang panimbang
Maskara Laban sa AlikabokMaskara Laban sa Alikabok
2

Grind for 3 hours in an iron ball mill

Grind the mixture for 3 hours in a mill with iron balls.

Mga kailangang kasangkapan:

Gilingang Bolang BakalGilingang Bolang Bakal
Maskara Laban sa AlikabokMaskara Laban sa Alikabok
3

Mould a ring at 4 tons per cm²

Mould a ring 3 cm across and 4 × 4 mm in section at 4 tons per square centimetre, with water as the plastifying and binding agent.

Mga kailangang kasangkapan:

Haydroliko na pandiinHaydroliko na pandiin
Dais na Pang-Press ng SingsingDais na Pang-Press ng Singsing
Distiladong TubigDistiladong Tubig
4

Fire 1 hour at 1050 °C, hold 14 hours at 600 °C

Sinter the ring in oxygen at 1050 °C for 1 hour, cool it slowly to 600 °C and hold it there for 14 hours, all in oxygen, then let it cool further. Snoek's core had an initial permeability of 385.

Mga kailangang kasangkapan:

Hurnong TuboHurnong Tubo
OksihenoOksiheno
Tangke ng gas na may presyonTangke ng gas na may presyon
PirometroPirometro
Sipit ng KrisolSipit ng Krisol
Guwantes na Matibay sa InitGuwantes na Matibay sa Init

Mga Materyales

4

Mga Kinakailangang Kasangkapan

12

Ang blueprint na ito ay gumagawa ng

CC0 Pampublikong Domain

Ang blueprint na ito ay inilabas sa ilalim ng CC0. Malaya kang kumopya, magbago, mamahagi, at gumamit nang walang pahintulot.