Ferrite Toroid Core: Copper-Zinc Ferrite by the Wet Process, Precipitated with Caustic Soda (Snoek 1948)

Snoek's copper-zinc ferrite made the wet way: copper, zinc and iron salts thrown down together with hot caustic soda, so the particles are very fine and pure. The washed deposit is pre-heated, pressed into a ring and fired in oxygen, with a 30-hour hold at 600 °C. His core reached an initial permeability of 500. Source: J. L. Snoek, US 2,452,529 (Philips, 1948), Example II, wet process. Picture: our diagram.
Abantado
3 days

Mga Tagubilin

1

Dissolve the copper, zinc and iron salts

Make 1 litre of a purified solution of 0.2 mol copper sulphate, 0.3 mol zinc sulphate and 1 mol iron nitrate. Ours: 49.94 g copper sulphate pentahydrate; weigh the zinc sulphate and ferric nitrate for the hydrate you have.

Mga materyales para sa hakbang na ito:

Copper sulfate pentahydrate (CuSO4·5H2O)Copper sulfate pentahydrate (CuSO4·5H2O)49.94 g
Zinc sulfateZinc sulfate0.3 mol
Ferric nitrateFerric nitrate1 mol
Distiladong TubigDistiladong Tubig1 l

Mga kailangang kasangkapan:

Timbangang panimbangTimbangang panimbang
Basong BorosilikatoBasong Borosilikato
Gwantes na gomaGwantes na goma
2

Precipitate hot with 9 M caustic soda

Heat the solution and precipitate it with 0.5 litre of 9 molar caustic soda. Ours: 180 g sodium hydroxide in water to 0.5 litre. Strong alkali: goggles and gloves.

Mga materyales para sa hakbang na ito:

Sodium Hydroxide — Uring PanlaboratoryoSodium Hydroxide — Uring Panlaboratoryo180 g

Mga kailangang kasangkapan:

Basong BorosilikatoBasong Borosilikato
Pang-init na PlatoPang-init na Plato
Salamin Laban sa Tilamsik ng KemikalSalamin Laban sa Tilamsik ng Kemikal
Gwantes na gomaGwantes na goma
3

Wash, dry and pre-heat at 700 °C

Wash out the deposit, dry it, and pre-heat it at 700 °C so it moulds better.

Mga kailangang kasangkapan:

Papel na PansalaPapel na Pansala
Distiladong TubigDistiladong Tubig
Hurnong pantuyoHurnong pantuyo
Hurnong TuboHurnong Tubo
Krisol na may takip (porselana)Krisol na may takip (porselana)
Guwantes na Matibay sa InitGuwantes na Matibay sa Init
4

Mould a ring at 4 tons per cm²

Mould the powder at 4 tons per square centimetre into a ring 3 cm across with a 4 × 4 mm section.

Mga kailangang kasangkapan:

Haydroliko na pandiinHaydroliko na pandiin
Dais na Pang-Press ng SingsingDais na Pang-Press ng Singsing
Maskara Laban sa AlikabokMaskara Laban sa Alikabok
5

Heat 3 hours at 900 °C, cool to 600 °C, hold 30 hours

Heat the ring for about 3 hours at 900 °C, cool it to 600 °C at 5 °C per minute, hold it there for 30 hours and let it cool to room temperature, all in a current of oxygen. Snoek's core: initial permeability 500.

Mga kailangang kasangkapan:

Hurnong TuboHurnong Tubo
OksihenoOksiheno
Tangke ng gas na may presyonTangke ng gas na may presyon
PirometroPirometro
Sipit ng KrisolSipit ng Krisol
Guwantes na Matibay sa InitGuwantes na Matibay sa Init

Mga Materyales

5

Mga Kinakailangang Kasangkapan

18

Ang blueprint na ito ay gumagawa ng

CC0 Pampublikong Domain

Ang blueprint na ito ay inilabas sa ilalim ng CC0. Malaya kang kumopya, magbago, mamahagi, at gumamit nang walang pahintulot.

Suportahan ang Maker sa pamamagitan ng pagbili ng mga produkto sa kanilang Blueprint Komisyon ng Maker itinakda ng mga Vendor, o lumikha ng bagong bersyon ng Blueprint na ito at isama bilang koneksyon sa iyong Blueprint upang ibahagi ang kita.

Talakayan

(0)

Mag-login upang sumali sa talakayan

Naglo-load ng mga komento...