Ferrite Toroid Core: Magnesium-Zinc Ferrite Fired at 1300 °C in Oxygen (Snoek)
Charlie

Nilikha ni

Charlie

21. Oktubre 2026DE
15
0
0
0
0

Ferrite Toroid Core: Magnesium-Zinc Ferrite Fired at 1300 °C in Oxygen (Snoek)

Ferrite is a ceramic magnet: iron oxide combined with other metal oxides, carrying magnetic flux while hardly conducting electricity. Snoek at Philips (US 2,452,531, 1948) made this magnesium-zinc ferrite ring: magnesia, zinc oxide and iron oxide ground together, moulded with water into a ring and fired in oxygen at 1300 °C for 1 hour, then cooled slowly. His ring had an initial permeability of 350. The picture: our diagram.
Abantado
1 day

Mga Tagubilin

1

Mix 26.5 : 26.5 : 47 mol

Mix pure magnesium oxide, zinc oxide and iron oxide in the molecular ratio 26.5 : 26.5 : 47. Ours, by weight: 9.95 g magnesium oxide, 20.10 g zinc oxide and 69.95 g ferric oxide per 100 g.

Mga materyales para sa hakbang na ito:

Oksido ng magnesiyoOksido ng magnesiyo9.95 g
Pulbos ng Zinc OxidePulbos ng Zinc Oxide20.1 g
Ferric oxideFerric oxide69.95 g

Mga kailangang kasangkapan:

Timbangang panimbangTimbangang panimbang
Maskara Laban sa AlikabokMaskara Laban sa Alikabok
2

Grind for 3 hours in an iron ball mill

Grind the mixture for 3 hours in a mill with iron balls.

Mga kailangang kasangkapan:

Gilingang Bolang BakalGilingang Bolang Bakal
Maskara Laban sa AlikabokMaskara Laban sa Alikabok
3

Mould a ring at 4 tons per cm²

Mould a ring 3 cm across and 4 × 4 mm in section at 4 tons per square centimetre, with water as the plastifying and binding agent.

Mga kailangang kasangkapan:

Haydroliko na pandiinHaydroliko na pandiin
Dais na Pang-Press ng SingsingDais na Pang-Press ng Singsing
Distiladong TubigDistiladong Tubig
4

Fire 1 hour at 1300 °C, cool at 3 °C a minute

Heat the ring in oxygen to 1300 °C for 1 hour, then cool it in oxygen at about 3 °C per minute. Snoek's ring had an initial permeability of 350.

Mga kailangang kasangkapan:

Hurnong TuboHurnong Tubo
OksihenoOksiheno
Tangke ng gas na may presyonTangke ng gas na may presyon
PirometroPirometro
Sipit ng KrisolSipit ng Krisol
Guwantes na Matibay sa InitGuwantes na Matibay sa Init

Mga Materyales

3

Mga Kinakailangang Kasangkapan

12

Ang blueprint na ito ay gumagawa ng

CC0 Pampublikong Domain

Ang blueprint na ito ay inilabas sa ilalim ng CC0. Malaya kang kumopya, magbago, mamahagi, at gumamit nang walang pahintulot.