Ferrite Toroid Core: Magnesium-Zinc Ferrite, One-Day Grind, 1400 °C (Snoek 1948, Ex. II)

A soft ferrite ring core of magnesium-zinc ferrite: magnesia, zinc oxide and iron oxide ground for a whole day, pressed into a ring and fired at 1400 °C in oxygen. Snoek's ring had an initial permeability of 670 and a Curie point near 100 °C. Source: J. L. Snoek, US 2,452,530 (Philips, 1948), Example II. The violet iron oxide has its own blueprint (precipitated hematite calcined at 1000-1100 °C, after Nurdini et al. 2022); Snoek does not say how his was made. Picture: the patent's Fig. 4, the ring core.
Abantado
2 days

Mga Tagubilin

1

Weigh 25.5 : 25.5 : 49 mol %

Mix 25½ mol % pure magnesia, 25½ mol % pure zinc oxide and 49 mol % pure violet iron oxide. Ours, by weight: 9.4 g magnesium oxide, 18.99 g zinc oxide and 71.61 g iron oxide per 100 g. Snoek does not say what makes it 'violet'; violet iron oxide has its own blueprint.

Mga materyales para sa hakbang na ito:

Oksido ng magnesiyoOksido ng magnesiyo9.4 g
Pulbos ng Zinc OxidePulbos ng Zinc Oxide18.99 g
Lilang iron oxideLilang iron oxide71.61 g

Mga kailangang kasangkapan:

Timbangang panimbangTimbangang panimbang
Maskara Laban sa AlikabokMaskara Laban sa Alikabok
2

Grind for one day in an iron ball mill

Grind the mixture for one day in a mill with iron balls.

Mga kailangang kasangkapan:

Gilingang Bolang BakalGilingang Bolang Bakal
Maskara Laban sa AlikabokMaskara Laban sa Alikabok
3

Press a ring at 4 tons per cm²

Press the powder at 4 tons per square centimetre into a ring 3 cm across with a 4 × 4 mm cross-section.

Mga kailangang kasangkapan:

Haydroliko na pandiinHaydroliko na pandiin
Dais na Pang-Press ng SingsingDais na Pang-Press ng Singsing
Maskara Laban sa AlikabokMaskara Laban sa Alikabok
4

Fire 1 hour at 1400 °C, cool slowly in oxygen

Heat the ring in oxygen for 1 hour at 1400 °C, then cool it slowly in oxygen. Snoek's ring had an initial permeability of 670 at room temperature and 2 kHz.

Mga kailangang kasangkapan:

Hurnong TuboHurnong Tubo
OksihenoOksiheno
Tangke ng gas na may presyonTangke ng gas na may presyon
PirometroPirometro
Sipit ng KrisolSipit ng Krisol
Guwantes na Matibay sa InitGuwantes na Matibay sa Init

Mga Materyales

3

Mga Kinakailangang Kasangkapan

11

Ang blueprint na ito ay gumagawa ng

CC0 Pampublikong Domain

Ang blueprint na ito ay inilabas sa ilalim ng CC0. Malaya kang kumopya, magbago, mamahagi, at gumamit nang walang pahintulot.

Suportahan ang Maker sa pamamagitan ng pagbili ng mga produkto sa kanilang Blueprint Komisyon ng Maker itinakda ng mga Vendor, o lumikha ng bagong bersyon ng Blueprint na ito at isama bilang koneksyon sa iyong Blueprint upang ibahagi ang kita.

Talakayan

(0)

Mag-login upang sumali sa talakayan

Naglo-load ng mga komento...