Ferrite Toroid Core: Magnesium-Zinc Ferrite Reheated 18 h at 1000 °C and 20 h at 750 °C (Snoek 1948, Ex. III)
Charlie

Nilikha ni

Charlie

28. Oktubre 2026DE
10
0
0
0
0

Ferrite Toroid Core: Magnesium-Zinc Ferrite Reheated 18 h at 1000 °C and 20 h at 750 °C (Snoek 1948, Ex. III)

Snoek's magnesium-zinc ferrite ring (Example III), fired at 1400 °C and then given a second long treatment in oxygen: 18 hours at 1000 °C and 20 hours at 750 °C. He measured how its losses change with frequency, but gives no permeability for the reheated core. Source: J. L. Snoek, US 2,452,529 (Philips, 1948), Example III. Picture: our diagram.
Abantado
3 days

Mga Tagubilin

1

Weigh 28 : 18 : 54 mol %

Mix 28 mol % magnesium oxide, 18 mol % zinc oxide and 54 mol % ferric oxide. Ours, by weight: 10.06 g magnesium oxide, 13.06 g zinc oxide and 76.88 g ferric oxide per 100 g.

Mga materyales para sa hakbang na ito:

Oksido ng magnesiyoOksido ng magnesiyo10.06 g
Pulbos ng Zinc OxidePulbos ng Zinc Oxide13.06 g
Ferric oxideFerric oxide76.88 g

Mga kailangang kasangkapan:

Timbangang panimbangTimbangang panimbang
Maskara Laban sa AlikabokMaskara Laban sa Alikabok
2

Grind 30 hours in an iron mill

Grind the mixture for 30 hours in an iron ball mill.

Mga kailangang kasangkapan:

Gilingang Bolang BakalGilingang Bolang Bakal
Maskara Laban sa AlikabokMaskara Laban sa Alikabok
3

Mould a ring at 4 tons per cm²

Mould the powder at 4 tons per square centimetre into a ring 3 cm across with a 4 × 4 mm section.

Mga kailangang kasangkapan:

Haydroliko na pandiinHaydroliko na pandiin
Dais na Pang-Press ng SingsingDais na Pang-Press ng Singsing
Maskara Laban sa AlikabokMaskara Laban sa Alikabok
4

Fire 2 hours at 1400 °C, cool 5–10 °C a minute

Heat the ring in oxygen for 2 hours at 1400 °C and cool it slowly in oxygen at 5 to 10 °C per minute.

Mga kailangang kasangkapan:

Hurnong TuboHurnong Tubo
OksihenoOksiheno
Tangke ng gas na may presyonTangke ng gas na may presyon
PirometroPirometro
Sipit ng KrisolSipit ng Krisol
Guwantes na Matibay sa InitGuwantes na Matibay sa Init
5

Reheat: 18 hours at 1000 °C, 20 hours at 750 °C

Heat the cooled core to 1000 °C and hold it there for 18 hours, then at 750 °C for 20 hours, and cool slowly again, all in oxygen. Snoek shows the resulting losses only as a curve; he gives no permeability for it.

Mga kailangang kasangkapan:

Hurnong TuboHurnong Tubo
OksihenoOksiheno
Tangke ng gas na may presyonTangke ng gas na may presyon
PirometroPirometro
Sipit ng KrisolSipit ng Krisol
Guwantes na Matibay sa InitGuwantes na Matibay sa Init

Mga Materyales

3

Mga Kinakailangang Kasangkapan

11

Ang blueprint na ito ay gumagawa ng

Kaugnay na Blueprint

Ang mga blueprint na ito ay nagbabahagi ng kaalaman — mga teknik, materyales, o prinsipyo

CC0 Pampublikong Domain

Ang blueprint na ito ay inilabas sa ilalim ng CC0. Malaya kang kumopya, magbago, mamahagi, at gumamit nang walang pahintulot.

Suportahan ang Maker sa pamamagitan ng pagbili ng mga produkto sa kanilang Blueprint Komisyon ng Maker itinakda ng mga Vendor, o lumikha ng bagong bersyon ng Blueprint na ito at isama bilang koneksyon sa iyong Blueprint upang ibahagi ang kita.

Talakayan

(0)

Mag-login upang sumali sa talakayan

Naglo-load ng mga komento...